Subject: Re: Glazing large flat areas

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Glazing large flat areas

9/30/15       
Kevin Member

I am having a heck of a time glazing over white cv without it looking splotchy. This job is matching some factory cabs and I just can't get the large areas (i.e. end panels) to look even. I have done the face frames and they look fine. I have tried a washcoat over the white, as well as thinning the glaze more and more with minereal spirits, but just can't get it perfect. I wipe on/wipe off as fast as humanly possible, but no luck. The cab panels done at the factory have NO streaks or splotching. Any advice? Thanks.

9/30/15       #2: Glazing large flat areas ...
JeffA

You could try and make a shader to match the color. I have done this for large flat panels and it has worked. Just watch for the overspray build up if there are corners.

9/30/15       #3: Glazing large flat areas ...
Robert Member

If you are making up your own glaze, will you post the ingredients ?

9/30/15       #4: Glazing large flat areas ...
Kevin Member

Thanks for the responses. I was actually thinking along the same lines as Jeff, trying to get an off white cv made that matches the color of the white/glaze combo. The glaze and cv is direct from from the cabinet manufacturer. Could not obtain the brand or ingredients from their tech support.

9/30/15       #5: Glazing large flat areas ...
ThomasFR

Kevin, try a few drops (or more) of boiled linseed oil to the reduced glaze. work on test panels to see of new mix is receptive to top coat. May require longer dry time before top coat. Good luck.

9/30/15       #6: Glazing large flat areas ...
Paul Snyder  Member

Kevin,

Are you glazing the entire surface with a uniform coat of color? Or are you wiping the glaze to let it hang up in the profiles? Not sure what you mean by splotchy...?

How are you applying the glaze? How long do you let the CV set-up before glazing?

If you're trying to get a uniform layer of glaze color then applying it like a toner with a spray gun will work. I think that's what JeffA has in mind. Since you don't know the properties of the glaze, you should sandwich it between coats of catalyzed vinyl sealer to be safe.

Sounds like you skipped the test samples stage, including an adhesion test.

9/30/15       #7: Glazing large flat areas ...
Kevin Member

The goal is a uniform coat of glaze color on the flat areas, with some hang up in the details (beaded face frames in this case). The glaze clearly alters the original color, but is only noticably present in the details where it hangs up. I am applying with a brush in the details, then using a rag on the flat areas. This is where the "splotchiness" comes in. Looks like areas just didn't get wiped back off evenly enough. I am following a glazing schedule recomended by my chemcraft guy, which doesn't involve vinyl sealer. I allow the CV to dry one hour, then glaze, let that dry one hour, then topcoat.
I did multiple test boards, including a cross hatch test for adhesion. Just didn't do a big enough board I guess.

9/30/15       #8: Glazing large flat areas ...
Kevin Member

Forgot to mention that I also tried it with a clear washcoat over the color coat. Better results, but not perfect.

9/30/15       #9: Glazing large flat areas ...
Zach Froble  Member

Website: http://www.lyndandesigns.com

I use a product from the autobody supply house that is a surface prep. It cleans up the excess glaze but does not affect the pigmented cv. Cleans up any unwanted glaze that has dried or smeared. Give it a shot and test with your topcoat. I have used a few different brands with no problems.

Zach

9/30/15       #10: Glazing large flat areas ...
chad

It sounds like you are saying it is drying before you can even the glaze out. Try wiping the surface with a mineral spirits after the glaze has dried.

9/30/15       #11: Glazing large flat areas ...
joe

kevin,

Your not allowing enough time for you base coat to dry prior to applying your glaze....the Chemcraft guy is giving you bad advise... What brand glaze are you applying some can be aggressive and will tend to bite on films that are not quite dry enough, others with slower oils not so much...I would break your system down with base coating one day and allowing an overnight dry then Glaze the following morning you will have much better results

9/30/15       #12: Glazing large flat areas ...
Lyndon

I agree with joe. You are getting bad advice. Your CV needs to dry overnight before you apply the glaze. What you are seeing is the glaze "biting" in some areas and not in others. Letting the CV dry overnight will make a difference. Also are you using dry or wet glaze?

10/1/15       #13: Glazing large flat areas ...
Paul Snyder  Member

Kevin.

Here's an alternative.

After glazing the profiles you can apply the color to the rest of the surface by making a thin toner/shader. Take a little of the glaze and reduce it with the thinner you usually use with your clear coat. Then add a little of the clear coat to act as a binder.

For example, start with this mix and adjust the amount of glaze you use to get the right color;

  • 1 oz. of glaze
  • 24 oz. of thinner
  • 6 oz. of clear coat

Do a spray test to see if you need to add more glaze or reduce it more. The nice thing about making it very thin (very little finish) is you can add more than one coat without building up a thick film.

If you get the color just right and are confident in your spray technique, you can skip the toner and just add the color to your final clear coat. You will need to add some thinner to the glaze before mixing it in with the clear coat just to make it compatible. This approach will save the added work of spraying a toner and separate topcoat.

If you're committed to applying the glaze by hand, the trick is to keep the entire surface wet long enough to wipe the glaze evenly. That means your rag will need to be pretty wet and you'll have to experiment with how much mineral spirits you need. Applying the glaze with a spray gun before you wipe it makes it easier - you start with an even wet layer and work from there.

10/1/15       #14: Glazing large flat areas ...
Kevin Member

Thanks all for the help. Using the glaze as a toner is a new one for me. Sounds like it might be the way to go. If I were to let the cv dry overnight, how do I scuff for adhesion(of topcoats) without the glaze highlighting the scratch pattern? That is something I've never had much luck with. Thanks again for all the input.

10/1/15       #15: Glazing large flat areas ...
Denny J

One thing that can help with keeping the glaze from biting in is to shoot a coat of clear over the pigmented prior to the glaze coat. Then shoot a final clear over that. This can all be done within the recoat window and gives a more even look.

Personally, for that type of thing I would look into something like MLCampbells amazing glaze. You can spray that on and take off what you want after it dries which makes it easier to get a consistent look.
A few companies had a WB equivalent back during the glaze rage and that was all I used 90% of the time.

10/1/15       #16: Glazing large flat areas ...
Jim Conklin  Member

Website: http://www.jhconklin.net

We glaze table tops rather often. We tend to use a 'furniture glaze' consistency. More like a thick stain than a syrup - thin enough to spray.

Four things have helped get it even.

1. Spray it on - gets things covered fast and evenly.

2. A fast dirty rag wipe to get the bulk off.

3. A spritz bottle of mineral spirits and a wide wallpaper brush to stroke out the smears. We brush initially in a chevron pattern, then finish along the grain (or the length, whatever.) Pressure on the brush tends to influence how much glaze hangs. As the brush loads, rub the build up off on a clean rag. As the glaze tacks and starts to grab too much, use the spritzer to keep it fluid.

4. If too much color use a pink Mirlon abrasive pad to stroke up some of the glaze. We've done this after 5 minutes and up to 5 hours after applying the glaze.

10/2/15       #17: Glazing large flat areas ...
JeffA

Just a note if using glaze as a shader. Make sure you strain it, glazes don't always have a fine grind of pigments to use as a shader. From experience.

10/2/15       #18: Glazing large flat areas ...
Matt Calnen

Last shop i worked at we used kerosene as a thinner to give better working properties for large areas

10/4/15       #19: Glazing large flat areas ...
Mike Fuson

I've posted the same question here before. I used to glaze over pigmented precat with dirty splotchy results and although I never had a complaint I really wanted a cleaner look. Through the help of guys on here I learned that the glaze was biting into the paint. The vinyl washcoat that some told me to do didn't work for me but a washcoat of cv did. It sealed the paint so that the glaze doesn't bite. On larger areas I do like chad said and sprits a little mineral spirits on it and go back over it again to lighten it up and even it out.

10/10/15       #20: Glazing large flat areas ...
Bart

@Kevin, Lots of good advice you're getting here. As for the scuffing. I always sand with 400 then scotchbrite (purple) real good with the grain.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)