Sawing and Drying

You are not logged in. [ Login ] Why log in
(NOTE: Login is not required to post)

White oak crossgrain and better cutting.

1/3/17       
fallguy Member

I have a good sized stack of white oak 600bf lumber and when I planed it, I really struggled with planer tear out. I am running an older foley-belsaw 5hp planer on 220v at its lower feed rate. I replaced the knives, but the tearout continued. When we followed with some walnut for a test, the quartersawn walnut planed perfectly. Now, the white oak trees or bur oaks? around here have lots of lower branches that spider off the tree and I'm guessing those spider branches are the source of the crossgraining, but the white oak was cut by a different sawyer that did not quarter much (sadly). The good news is most all the lumber planed down to 0.875", so I have some room to pick a good side to clean up. Question is, do I have to run these all through a sander instead of planing? On the same subject, but a little different, should a sawyer be lining up the pith in white oak and cutting the pith into something like a 4x4? Most of the pith wood really was impossible to finish nicely and even though air dried slowly under a cover still cracked up. Is some of this on the sawyer? I paid a sawyer and was a little frustrated that he didn't quartersaw more and level the logs to cut out the pith. Is it just me or is it a little criminal to flatsaw white oak? Some of the boards were 14" wide, and I ended up throwing the whole board out because it simply would not have made much. It is long past the time I would talk to the sawyer, but he was in a hurry to get in and out in a day and I got a lot of not very nice lumber as a result. How do you avoid a bad contract sawyer? His rate was 75/hr. and I never asked him to hurry at all. How can you avoid this with a sawyer and how should large white oak logs be sawn in general and any advice for the cranky/grainy flatsawn lumber I have? (and I realize some of flatsawn lumber is rift and quartered, etc) This is meant to be educational and for me to verify my suspicion/attitude that this wood was not cut very well.

1/5/17       #2: White oak crossgrain and better cut ...
Gene Wengert-WoodDoc

Tearout is caused by several factors, oftentimes two factors tHat individually not an issue but together they are a problem...2+2 = 8.

Low MC (under 6.5% MC), knife angle is too slender, rake angle is too large (determined by the head), knives not all in the same cutting circle, too much land (too much jointing), knives not sharp, feed too fast and removal rate (depth of cut) too large, too much swirly grain, wood not held firmly.

1/5/17       #3: White oak crossgrain and better cut ...
fallguy Member

MC was 13%, knife changes yielded no difference, graining was very swirly... I think it is just one of those times when the wood didn't cooperate. The feed rate slower might have reduced the tearout, but I was going as slow as the machine would go..

Thanks.

1/9/17       #4: White oak crossgrain and better cut ...
steve n


The best cure is a byrd spiral head, cost a lot but if you do a lot of planning well worth the cost. Steve

1/10/17       #5: White oak crossgrain and better cut ...
Eric Steadle

Let me talk to the sawyer part....

Lumber should be sawn for how it's going to be used. If your sawyer didn't ask you what you plan to do with the lumber, or what you want out of the logs he's sawing, you should have told him. If he told you something else, or that he couldn't do it, then that's the time to call someone else.

White oak makes great trailer decking, fence rails, barn flooring, and other outdoor use lumber. In those situations it is often flat sawn. And while white oak makes excellent quarter-sawn lumber too, it takes a lot of effort and skill to quarter saw, and not all sawyers are up to it. And not all customers are willing to pay for it. Quartering also reduces the overall yield of a log so you end up with less usable lumber.

1/19/17       #6: White oak crossgrain and better cut ...
Dave Boyt  Member

Website: http://www.pottershophollow.com

If you didn't communicate with the sawyer what you wanted, then there is no reason to blame him. Quarter sawing takes at least half again as much time as flat sawing, and has no advantage for many applications. The sawyer was probably just trying to give you the best value for your money. Another thing that might help is ripping the wider boards before planing, then edge gluing them back together. This is a common practice that helps relieve stress, as well as giving better yield if the boards are cupped. I agree about the spiral head idea.

1/19/17       #8: White oak crossgrain and better cut ...
fallguy

So, defending the sawyer.

Is it a good practice to run heartwood in multiple boards, or a better practice to dog the log and cut to remove the pith?

When I asked the sawyer about dogging the logs to get the pith in one board, he said he'd have to work an extra day and he was only going to be there for one day. Probably should have fired him right then eh?

Is it a good practice to cut 14" wide boards? I threw all boards of that log but 3 away as they were too cupped and rounded and facebowed to do anything with. Then my yield from the 3 boards was literally about 6 bf.

My original question was somewhat about whether quartersawing would have resulted in less crossgraining and tearout.

The spiralhead was probably the best answer.

Thanks all.

1/28/17       #9: White oak crossgrain and better cut ...
Steve McGuire

Just saying:
I contract saw for a long established white oak sawmill with my mobile sawmills. Quarter sawn boards are less susceptible to bowing and cupping, if they are clear. Put a knot anywhere and your going to have uneven movement no matter who cut the boards or how they are cut.
If the boards cut have too much slope of grain (see grade book) it can cause problems the strength of the board, in drying straight and maybe in planing (that's a guess).
Wide boards that contain wood from both sides of center will (tend) to cup opposite to the curvature of the grain. It's a physical thing due to the different ratios of summer wood and winter wood (light rings dark rings). If you rift cut a 2" x 2" it will not dry square no matter what. It will dry as a parallelogram because of the different shrinkage rates of the two growth periods.
If the heart center (pith) is in a board it will split, best to cut it out before drying.
Boards are all sawn flat it's the care and feeding (drying) that makes or breaks you.
Good stickering and lots of weight (like tons) are what most mills use to prevent problems. And some wax sealing the ends is also used.
One trick I've learned recently is to cut through and through, sticker with dry 1 1/2" x 1 1/2" stickers, throw out the top and bottom boards so you have flat surfaces, then band with poly strapping as tight as you dare. Waxing the ends will reduce end checking and the stickered log will stay straight as it dries. Store each bundled log in a shady place with air flow but not direct wind. If you leave a tail on the straps you can go back and re-tighten if they get loose.

1/28/17       #10: White oak crossgrain and better cut ...
Fallguy

Slope of grain was precisely what I was wondering about; didn't know the reference. Thanks! Where can I find out more about it? Every board I have would have it, save the walnut cut by another sawyer.

1/29/17       #11: White oak crossgrain and better cut ...
Steve McGuire

Slope of grain is more for strength in construction grades (conifers), not appearance grades (mostly hardwoods and some soft wood).
Western construction grades must have a slope of grain no more than 1 in 12. I don't have a grading book for hardwoods so don't know if that even applies. Where I live there is no applicable hardwood grading book. I do know that some hardwoods are cut cross grain on purpose to reveal more dramatic grain patterns such as cathedral. And some hardwoods you can't get away without cutting cross grain because of the way the log twists and turns. If you don't have a straight log the grain jumps all over the place. Such logs have a lot of tension in them and just want to twist and turn when cut. Best to cut twisty logs into thick beams and planks. To get good lumber you need good logs. But as a sawyer I don't get to pick which logs to cut, that's up to the log owner.

1/29/17       #12: White oak crossgrain and better cut ...
Gene Wengdsert-WoodDoc

SOG (slope of grain) does apply to the top grades of hardwoods in that end spilts cannot deviate more than 1:12. This applies to FAS, FAS 1-Face, and Select grades.

Indirectly, it applies to all grades in that SOG can cause warp and warp is a serious defect.

When one planes "against the grain" then chipped grain is more likely, but if planing one piece of lumber with the grain, the other side will be against the grain unless the lumber is turned end for end...not possible in medium and larger operation. So, we use chip breakers in -layers that are adjust precisely so that chipped grain can be avoided.

As stated earlier, the MC and drying temperature are likely the biggest factors affecting the development of chipped grain.

1/29/17       #13: White oak crossgrain and better cut ...
Fallguy

The MC of the 3 year air dried Minnesota in November batch was 12-14%. We had nearly zero checking, except near pith.

It would have been really hard to run each board with an sog reference, but I suppose I could have blackmarked each end for grain direction off center. I marked defects on the face with a crayon and check mark the board if none. It would be a lot of looking, flipping, spinning, and I like to run end to end...

At this point, I'm crediting swirly grain, planer speed (running slowest but still plenty fast), knive angles, knife type, and slope of grain a bit, kind of in that order. I hogged very lightly to the point my offbearer was getting a little mad at me. That caused the most frustration because a 0.030 hog still was tearing.

Thanks to everyone for responding. I learned plenty and am grateful.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)