I have seen many disparaging remarks in various forums about gorilla glue / polyurethane glue. Just curious why? It is contrary to my experience. I have used it many times for various applications from bent laminations with no springback to exterior application with great success. Why are many opposed to it's use?
From contributor Mi
Gorilla glue is for hacks.
From contributor Mi
And before somebody complains about what I had to say.
There is a time and place where polyurethane glues may be the best choice, however 99% of the time they are not. There is almost always a better choice. That may be PVA, Epoxy, UF, Plastic Resin, etc... In almost every application I can think of where "gorilla glue" may work there is probably a better choice.
I am pretty discussed with the way Gorilla glue is marketed as the "toughest glue on the planet" If I had an application where a polyurethane glue of that type were ideal, I would not buy gorilla glue. I would purchase another brand that does not overstate their product.
From contributor Ni
I'm with you Peter, it definitely has a time and a place, in fact I just recommended it to someone else who was trying to glue stainless trim to pt. bd.
It's not something I use very often (probably 6 times a year) as I absolutely hate working with it, but it's hard to argue its adhesion with certain materials. In fact when I run into one of those situations where I'm asking myself how on earth am I going to glue that??? The answer for me is generally gorilla glue.
And for all the nay-sayers out there, I have never had a situation where it has failed me. In fact the opposite is true, when other adhesives have let go its good old gorilla glue that comes to the rescue.
From contributor Le
For odd material adhesion I usually go with silicone.
If you want quick dry and waterproof under low stress joints I could see using GG. But I'd rather wait the time for an epoxy to dry.
From contributor Je
I pretty much agree with Mark that there's usually a better glue for any given application. Gorilla, (or Poly glues in general), are messy and just a real PITA to use. I come up with a use for it about once a year or so and have to go out and buy a small bottle since once you open one it'll harden up on you in several months:>(
JeffD
From contributor Ad
Gorilla type PUR glues are a modern adhesive. Some how we managed to do without them before they were invented.
Their ability to gap fill is absurd. Filling a gap full of foam that has no shear strength should not be compared to epoxy.
They are very expensive per volume. They go bad in about 6-12 months after opening the bottle.
They are by far the messiest adhesive I've had the pleasure of playing with.
The Gorilla Glue played no role in preventing spring back in your lamination.
The PURs excel at bonding dissimilar materials. Metal to wood is perhaps the best use for PUR adhesives.
You are confusing disparaging with the truth.
From contributor Mi
Also.
The gorilla type polyurethane resin glues are a niche adhesive suited for special applications.
Yet they seem to be marketed as a do everything product that is somehow the toughest glue in the world or something along that lines. Everybody who has any understanding of adhesives knows that this is not the case.
As mentioned above they are a poor woodworking glue, with exception to a few special circumstances (wet lumber might be an example) From my experience and that of my peers performance with exotic/oily woods is mixed but that is another situation where I have seen or heard of results that are reportedly better than other adhesives at times. However even that evidence is anecdotal at best and conflicting.
As a general purpose adhesive these gorilla type glues are no better. For general purpose applications 2 part epoxy, CA glue both come to mind. People who talk about failures with epoxy are either using them incorrectly, our outside of the manufactures guidelines. I won't let it stand that people tend to blame adhesives for their personal mistakes or inability to follow directions.
Now I do not mean to discount industrial PUR (polyurethane resin) adhesives, especially hot melt formulations. I frequently use the tightbond PUR hot melt system in my shop, and it works quite well for gluing any two things you can think of with little pressure.
From contributor La
Fine Woodworking Mag. did some glue testing and found Gorilla to be one of the weakest of the glues used for woodworking. Like others have said there are uses for PU's but as a general woodworking glue, not worth the cost or the mess. We have the 3M Hotmelt PU system, required by one of our customers to glue dissimilar materials. Rather expensive and I wouldn't buy it for general use.
From contributor Ji
My hands after using the product
From contributor Ad
Jim,
Have you considered making a claim against Gorilla? You could finally retire a rich man(with the hands of a gorilla).
You definitely have to wear off PUR when you get it on your hands. Not even aggressive solvents will touch it.
I honestly can't remember the last time I used a PUR. It's got to be almost 10 years.
I would not put the hot glue PUR in the same category as liquid PUR.
Gorilla itself deserves a bit of disdain simply for their marketing campaign. I hope they have made a ton of money. Their gorilla tape is pretty average as well. Kinda like thick cheap duct tape except it costs 3 times 3m tape.
From contributor Da
I once had an employee that would ask if we were going to use any Gorilla glue (back when we used it more than we do now) on Fridays.
After a few weeks of these questions, I asked him why. He said he was hoping to have sex with his wife Friday night (date night, babysitter, etc), but she would not let him touch her if he had the 'brown hands' from using Gorilla glue. I got him some disposable gloves and everyone was happy.
Jim - I'll send you some gloves if you like!
From contributor Mi
On a side note car mechanics have the whole disposable glove thing all figured out.
Get your car mechanic to order a case of gloves or find out what they use.
From contributor Ge
Great discussion indeed. I do believe that the discussion should indicate that much of what was said was in reference to a specific type of adhesive and not just to one brand. However, within the pur family, there are many adhesives formulations. That is, not all pur adhesives are the same.
Also, as we have said many times before, the wood strength in a properly made glue joint is the weakest link and not the adhesive. So having a stronger adhesive does provide little benefit in most cases. The strength of the joint depends on the wood surface preparation mainly.
From contributor B.
We use Franklin brand polyurethane glue on western red cedar and pretty much nothing else.
I did my own glue tests on western red cedar years ago and the polyurethane glue was the strongest. The process included wiping down the cedar with acetone (if I remember correctly) prior to glue up so as to remove oils from the surface.
Sometimes we will use West System on cedar as well but often times the dark glue line is not acceptable.
As mentioned polyurethane glue is also a good choice when working with wood to metal etc. And as others have mentioned we always wear vinyl gloves when using the stuff.
BH Davis
From contributor Ma
To Mark and all those bad mouthing Gorilla Glue - try leaving your cozy little world of kiln dried wood and super stocked US woodworking stores, go to another country like Panama, where all lumber is in block form, uneven humidity (or even wet) have tons of work to finish and you need to finish to feed your family - tell me of another glue that will allow you to unclamp humid wood in twenty minutes. GORILLA GLUE IS AWESOME. 90% of all the work on my site was glued up with it - www.bogazzi.com.
From contributor Jo
I normally don't use GG but a recent project it worked well on: Outdoor /indoor benches made from 2" thick wood slabs with drawknife shaped legs connected with wedged round tenons. The combination of wedges and expanding glue made for some strong, waterproof joints.

From contributor Ji
"GG" (godawful-goop)
I'm just having fun her in my "cozy little world". GG is not my favorite type of foaming suds but I do keep a bottle or two stashed away. Unfortunately is doesn't age too well and the last vintage had to be discarded.
Next time I find myself deep in the tropical jungle, I'll look for more gorilla-spore-glue
From contributor Ch
I have to say That I never had saticfactory results from GG and stopped even attempting to use it.
A few years ago I had the need to put some door frames together and wanted a water proof quick drying glue, And I found a pur glue that came in a silicon tube. it had gap filling, water proof and quick drying capabilities. it also acted like a lubricant so I could get the bridal joints together easy and was hard as a rock after only a few minutes.
Since then I use it on the odd occasion (mostly for doors and door frames) and am thrilled to have discovered it!
Chaim
From contributor Ge
GG name is used for several types of adhesives including a PUR, a PVA, an epoxy and a tape.
Gorilla Wood Glue is a PVA. Gorilla Glue is a PUR. I do wonder if some of the discussion has confused the two.
Would someone check the label to see if it has to be used with good ventilation? Is this because of carcinogenic risk? You can also check their site, linked below.
You will find some info on the Internet that says Gorilla Glue does not release vapors, etc, but that is for the Gorilla Wood Glue, a PVA. PVAs do not have such a warning, do they?
Note that there are three types of PUR adhesives: Hot melts (much better than the nylon hot melts of the past, so do not confuse them with the old stuff), cold application (as we discussed above) and two-part (somewhat similar to epoxy and this one does not need moisture to cure as one part is the "hardener").
Why use PUR? In general, it has a long open time (except in humid environments), bonds well to many materials, and does not have water (compared to PVA) so swelling is not an issue. It does take a long time (24 hours or more) for the strength to develop fully with PUR, especially with very dry wood. PUR does have the same issues with gap filling and wood with oils that PVAs have.
From contributor Ji
Actually Marc, I would love to hear more about living and working in Central America. I've heard similar stories or comments about having to work with rough, native lumber and under less than ideal conditions etc. I'd really like to know what it's like to work and live Central America? I've also heard that some areas may be good retirement destinations for North Americans?
As you may be aware, our cozy little North American world has become (in some respects) not all that cozy. The cost of health insurance and medical care for example, has literally gone through the roof! (At this point, I'd consider moving to Albania... wherever that is). I'm self-employed and my monthly insurance premiums (for two adults) now exceeds my home mortgage payment!
Anyway, perhaps I might persuade you to comment or start a new thread on the subject? I solemnly swear to STFU about GG .
From contributor Ge
The PUR adhesives were developed and used in Europe 35 years ago as a response to "no formaldehyde" adhesives. They were and are indeed available in much of the world (although they cost more than the adhesives used in the USA with the F word) for many years under various company trade names. The cold setting PUR work very well in humid environments.
Using a PUR requires a bit of a learning curve, and I suspect that often this is why one person has problems with them. Sometimes, they use a cheap PUR and then they wonder why they do not get good results. (I wonder if the PUR sold under one label in a foreign country is the same formulation that we have in the USA.) Like I also said, "Gorilla Glue" has different types, so Gorilla Wood Glue is a PVA and not a PUR.
Bottom line is that PUR has a lot going for it, when used properly. But it is more expensive.Oftentimes we do not need all the extra strength or whatever it offers, so why spend the extra money?
From contributor Da
Marco - I also am curious as to how woodworking is different in a humid/tropical climate. Around here (Midwest US), if wood isn't around 6-8% MC (interior work, hardwoods) it is liable to move as it gets down to the local EMC.
As we all (should ) know, one glue is not the answer for every use. Different woods, uses and joinery require different characteristics. Viva la difference!
So if your wood is less dry, then the local EMC must be higher. The items on your website (nice work, by the way) are not rustic, slapped together things but show a refinement of design and method that requires excellent joints. You really do show a lot of faith in the glue - as you say, your livelihood depends upon it.
I always liked the way the GG worked - good sanding, easy clean up, once cured, and long open time. I was put off by strength tests that showed a lower strength in various joints than other glues.
From contributor B.
David,
I have to confess I did not go to Marco's website when I responded to this issue. Sometimes I take a minute and look at a poster's business site and sometimes I just push on to the next task at hand. I should have spent a few minutes with Marco.
Marco,
Really great design and construction. We all see a lot of photos of other peoples work here on Woodweb. Much of it is worthy of a longer and more studied look. In my opinion yours is right up there with the nicest of what I've seen over the years and definitely worthy of an extended visit to your website for some really great eye candy.
Thanks for sharing.
BH Davis
From contributor La
Marco, Very nice work and the perfect application for PUR.
From contributor Ma
Woodworking in Panama is like this:
Amazing variety of lumber - all of it is cut into manageable blocks (unfortunately, due to lack of large chainsaws, large diameter trees are cut up into smaller blocks) and dried as blocks.
So when I go to the sawmill, I am choosing amongst blocks, 90% of which are checked to varying degrees on the ends. You try to select the driest BLOCKS - they usually mix them up (dry blocks doesnīt get stacked to the top).
They cut your blocks to whatever thickness you want - worst thing is not only does every boards share the checks, every board has a different humidity - Iīve seen the first boards come off dry, bowing like frying bacon, and as they approach the middle of the block it stays flatter but is darker (wetter). Alot of times sun is on the blocks, which causes hugely uneven stresses.
After a few years of this you learn to select blocks of certain species which are not necessarily dry, but straight grained and whose movement is predictable. Then you design each piece and allow for movement in only one plane. It sounds horrific (and at times it was!) but it worked, if you respected wood movement and planned for it (the same way green wood chairmakers work).
After a few more years of dealing with this, the main problem to avoid was not wood movement, but ensuring that fungi didnīt develop.
At the end of the day when I would close the shop, I would have to sandwich the wood panels that I glued up earlier in the day between plywood, because if I didnīt the boards would be cupped the next day (they would dry a little on the exposed face). It was not the humidity in the air that affects the glue, its the humidity in the wood. That why I depended on GG.
I BECAME OBSESSED WITH FLATNESS!!! That was my greatest challenge, and had to learn how to deal with cupping, it was like a moving target.
I just moved to Atlanta and bought lumber and find myself employing habits that I developed in Panama for working humid lumber, and am SO relieved at the stability of the lumber here.
Yes, some say, "you shouldīve built a kiln", that is true, but drying my own lumber was not a luxury I could afford - isnīt drying lumber a business in and of itself?
From contributor Da
Interior woodwork SHALL be built from lumber that has been properly dried to an appropriate EMC suitable for the climate in which it will be installed.
Anything less only serves to lower the bar. You cannot simply build woodwork any way you desire from whatever material happens to be readily available. If you can't afford the necessary material, you cannot build and sell woodwork to the public.
As a professional you have a duty to uphold certain standards of quality. Such standards have been derived through science, and practical experience of many skilled tradesmen.
Anything short would be a disservice to the general public whom places trust in the professionals whom they deal with.
Suggesting the use of wet lumber for quality interior woodwork is uncalled for, and unprofessional, and deviates from what would be expected of someone with a basic understanding of woodworking.
It is one thing to use whatever is convenient for low quality rustic work and even that is questionable. However there are countless professionals who go to great lengths to do things the right way.
From contributor Ge
Dry kilns are a little over 100 years old. Prior to that time, kiln drying was not used even for fine furniture. In fact, kiln drying only became important when central heating was used.
When one is rich, one can define quality differently than when one has less money.
From contributor Da
In the past 100 years we have seen forced air heating systems and mechanical air-conditiong, and dehumidification systems. Furthermore standards of living have changed resulting in dehumidification in humid climates to reduced/prevent mold growth.
People who admit to using wet wood that has not even been properly air dried and seasoned, and then suggest band aid fixes for the resulting problems are not an asset to the trade.
From contributor Ma
I was only an asset to my clients, who to this day are enjoying their furniture.
From contributor Ni
Well now I just have to post on here again... Thanks again for mentioning gorilla glue on this site Peter, it's almost as bad as talking about melamine and joints other than dovetails.
There is a time and a place for everything. I don't use gorilla glue often, but it's not to be disregarded.
To you Marco, the furniture looks amazing, if they're your designs, I'll hold you in even higher regard.
To everyone else who may have lost their marbles over the subject, maybe take a trip down to panama and take a look at the material firsthand. Call me crazy, but I don't think he was using birch or maple down there.
In my experience, the exotic (to us) woods tend to grow a little differently. Generally taller as they're competing in more of a rainforest environment with very few limbs growing anywhere but near the top. Think more like the old growth fir we used here generations ago. Nice stuff, wasn't kiln dried, never really shrank.
In fact I still have lots of it in my home that's over 100 years old, and even with my a/c running in the humid summers, it refuses to shrink. Where as the mdf that I've put in the top floor, which was primed all 4 sides, glued at every joint, nailed into every stud moves around more than the dog.
From contributor Ch
I took a couple of pics of the adhesive I was talking about in my previous post.
I had hoped to find a link on the companies web site but had a hard time in Danish...lol
Its a good glue in certain applications, It doesn't foam too much and hardens within a few minutes and cures in 24 hours.
I would not use this in every circumstance but like I said for fitting door and door frames together this works great!
Chaim


From contributor Ma
Dave, here is an example - there are many US doctors who have very successful practices, all proceures are followed, they have all the latest tools and supplies. Those same doctors on ocassion will do volunteer trips abroad to areas that need medical attention - areas where they donīt have half the materials, supplies, and setup that they would here in the US and yet they save lives or make them better. Would you tell them that they are lowering the standards of their profession because they are doing this without the optimal setup they had in the US?
From contributor Da
The last time I checked Panama was not on the same level as Haiti or Somalia.
Drying wood is a basic skill that does not require sophisticated technology. A moisture meter should not be impossible to get unless your in North Korea.
From contributor Je
Dave, have you looked at his website? Have you seen his work? I think making assumptions that everyone should work the way YOU think is correct is a bit closed minded. There are countless shops in this country working with properly kiln dried woods that are making garbage.
Either you make quality work out of the materials at hand, or you don't. To imply that his work is any less quality based on such assumptions is unwise at best.
JeffD
From contributor Da
You must use quality materials.
From contributor Da
Anything less is not professional.
From contributor Je
Sorry Dave, but I think your still making a lot of assumptions. How would you establish the quality of the materials based on the method of drying? FWIW if you have a local museum with antique furniture on display....it was not kiln dried;>)
Now I could be wrong on this, but I'm thinking there's probably not a lot of central heating in Panama? So that point is probably moot?
Having been lucky enough to have done some traveling in different countries I've seen a lot of high quality work done with what was at hand. The fact that it's still there in some cases hundreds of years later, is a testament to that quality. No kilns, no CNC's or other expensive equipment, and no Gorilla glue....I'd still say it was done by professionals:>)
Anyway we can disagree I suppose, but you may want to at least consider the possibility that the whole world doesn't do things the way we do in our little corner of it;>)
good luck,
JeffD
From contributor B.
I was logging in to say exactly what JeffD has just expressed. Thank you Jeff.
I don't mean to be rude but the criticism being directed at a genuinely gifted craftsman producing projects that are obviously of the highest quality level in design and workmanship is totally misguided. Unless Marco is a complete fraud in his online portfolio..........which I doubt to be the case........his work is to be commended, not criticized.
One works with what one has at hand. To study and learn how to turn those less than ideal conditions into well built and long lasting products is the ideal we should ALL be striving towards. What impresses me the most about Marco's work is that he has studied and learned how to accomplish this goal with material that starts at such a less than ideal condition.
Kiln dried wood is not always the best answer in every situation. Ask any steam bender or turner what they want to start with for many projects. And as Dr. Wengert so accurately pointed out it is modern living conditions that dictate the need for the moisture content levels achieved by the kiln. If Marco has figured out a way to take the air drying process (which is giving him the needed moisture content level for Central America) from pre-construction to post-construction there is nothing at all wrong with that. Not many are willing to study a situation to the extent required to bring about a successful result under those conditons.
BH Davis
From contributor Da
Strident pronouncements and a commanded adherence to one person's world view do not a professional make.
In fact, we have all been humbled often by this material we profess to admire - even love. That humility has taught us all to open up, loosen up and find a way. This broadens our skills and knowledge in such a way that not only makes us better woodworkers, but enables a wider, more accepting view of the world around us.
Marco found a way to adapt to his tropical environment and still have the satisfaction of making fine objects, satisfying his clients and supporting his family - all very worthy achievements. He has not demanded my respect, but he certainly has it, and I can confidently call him a professional.
In short, I would invite anyone with such a different/radical view to post some photos to see if others would view that body of work as Marco's is viewed - and accepted. It certainly would be a better way to make one's point than to just lecture on fundamentals.
From contributor Jo
Dave,
First, let me say I have been involved in the woodworking profession for 40 years, building custom kitchen cabinetry and custom furniture for most of that time, along with a period of custom homebuilding and design. I have always strived to utilize the best materials available for the project on hand. That being said, most of the time I worked with air dried woods, harvested myself. A large percentage of those woods were not clear, select grade hardwoods but closer to a character grade as that was the look my customers loved. By your definition of only the best, I guess this was not very "proffesional" of me.
I wonder what some of the masters of our time, Sam Maloof, Tage Frid, George Nakashima, etc. would think of your rigid "rules"? I think it is much more important to understand the materials and know how to work with it's movements (All wood continues to move, even kiln dried wood) based on the enviroment it will be in. Marco seems to have accomplished this quite well. It's no different than someone building high end chairs from green wood as many highly skilled craftsman have for hundreds of years.
Second, while you have your right to your opinion, your comments were rude, vulgar, condescending, and have no place on this forum. There are ways to word your opinion that would have been more polite, you chose not to. Thankfully, most posters on this forum do not behave in this way. As to the original posted question, again, Gorilla Glue PUR is not my glue of choice but it does have it's place on my shelf.
From contributor Ge
Certainly, one can try to post their opinion without specifically attacking or degrading the opinion of another.
So, regarding PUR adhesives, let's look specifically at hot-melts.
I do think we could use PUR hot-melt adhesives much more often that we presently do. We often think that hot melts are weak, for hobbyists, etc. Here is a bit of info about PUR hot melts. They do more than just cool and get solid...like other PUR adhesives, they also react with moisture to form an awesome bond.
Hot-melt PURs are solid at room temperature, but when heated to 250 F, flow very well. These hot adhesives, when applied to the wood, then cool and begin to provide good joint strength within 15 seconds to 3 minutes, depending on the formulation. The fast curing and good initial strength can often eliminate the need for nails and screws.
But here is what is different. PUR hot-melts involve two different curing mechanisms: First, as the adhesive cools, it solidifies and provides good bonding (as in the past and stated above). But then, the adhesive cures further (over the next 24 to 72 hours) by reacting with moisture in the wood and air, thereby providing cross-linking of wood and adhesive molecules and the high strength of a PUR adhesive.
PURs are noteworthy in that they do not contain moisture themselves, so the wood-moisture interaction (like sunken joints or warped veneer) are not an issue. And of course, clean-up is so easy.
From contributor B.
We gave hot melt PUR adhesive a test trial on our segmented construction curved mouldings a few years back. I thought it might be an alternative to the WorkRite wood welder for speeding up the curing of the joints. Plus I wondered if it might hold butt joints tightly enough not to require additional joinery. As most we typically would not send something out that has no joinery in butt joints but the PUR looked like it might hold some promise in this area.
The PUR worked well enough in terms of ease of use and strength of the butt joint. However it would not form nearly as thin a glue line as anything else we use.
Also even with very tightly pressed joints we found a raised lip at all joints when profiled. It appeared the PUR compressed slightly as moulder knives passed over the joint and then expanded back upwards on the order of 128th of an inch (or even less).........just enough so you could feel a rubber like ridge at every joint. Sanding did not help.
That along with the inconvenience of having to bring the glue and applicator up to temperature with each intermittent use ruled it out as a reasonable option for us.
BH Davis
From contributor Je
Well the hot melt PUR's are a different animal than the foaming liquid goo like Gorilla glue. My problem with the PUR's was even using the ones with a longer open time there was so little time to assemble that it became too difficult to get pieces together quickly enough. For many of the things I glue up several minutes are need from start to tightening the last clamp.
I bought one of the hobby systems for something like $125 or so some years and I don't think I had it more than a year before I gave it away. It was handy for certain things, but many were things I could have done with a basic hot melt glue gun for much less $$$. I'm sure the pro systems would give much better results, but for the work I do plain old yellow glue proved to be the better solution for most things.
JeffD
From contributor Ge
When PVAs were first invented and marketed, they were white in color. When they were improved, the glue color changed to yellow. Not to be undone, some white glues added a yellow color too. So, today, the color does not indicate the type of PVA. So, when describing a PVA, it is possibly more helpful to add terms like "cross-linking" or even a trade name and number to indicate that it is a different adhesive than the old fashioned white PVA. Example: Consider the difference between TB, TB2 and TB3...all the same color and all PVAs, but properties are quite a bit different.
From contributor Je
Good point, and I'll just mention that I personally wouldn't mind if TB1 went back to white. There are certain applications where the clear glue line would be advantageous over the current yellow flavor;>)
JeffD
From contributor La
We've got the 3M PUR hot system. It holds well and works to hold other materials to wood but does produce thick, by comparison, glue line. The working time even with the longest formulation is short compared to PVA. The longer it is left unclamped, if you are using it where it can be clamped, the thicker the glue line even if it is still with in the allowed time. So best used where you have "non-flush" joining. The gun, about $700+, the 4 tube preheater? can't remember the price, and the $70+/ 10oz. tube of glue, in case lots, certainly discourages much use.
From contributor Ge
Larry is indeed right on target.
I do have one cabinetmaker client that uses hot melts for frame assembly. They get the pressure on within 10 to 12 seconds after glue application in order to avoid too thick a joint. They really like the slight flexibility of the joint, the ease of clean up of squeeze out, and the short clamp time. After 12 hours, they think the strength is comparable to PVAs and after 72 hours, it is much better. They are gluing some miter joints with some end grain characteristics, but not 100% end grain. I do not know their cost numbers, but the speed of assembly and the reduced repairs offset the higher cost, they say.
From contributor St
Full Disclosure: I'm a new advertiser here, and a chemist; my company manufactures epoxy adhesives and related things. This post has absolutely nothing to do with that.
I was looking thru this thread, and came to the picture of Jim Baldwin's hands.
Please do not do that. Wear rubber gloves, no matter how
uncomfortable, when using Gorilla Glue or other polyurethane
adhesives. They contain isocyanates, which are sensitizing agents; One
can become *sensitized* and then hypersensitive after some
indeterminate amount of exposure to isocyanates, and then cannot go
anywhere near them without a *strong* allergic reaction. It is a genetic
thing, with those of fair skin and/or reddish hair the most prone to
become sensitized.
Gorilla Glue contains methylene diphenyl diisocyanate monomer and
polymer. Dried, after full polymerization, it is harmless (unless you
burn it; then it liberates small amounts of highly toxic things, as
does most stuff). HOWEVER, in the liquid state, here is what you
should see on the MSDS and expect in real life:
EXPOSURE GUIDELINES:
Medical supervision of all employees who handle or come in contact
with respiratory sensitizers is recommended. Persons with respiratory
problems including asthmatic-type conditions, chronic bronchitis,
other chronic respiratory diseases or recurrent skin eczema or skin
allergies should be evaluated for their suitability of working with
this product. Once a person is diagnosed as sensitized, no further
exposure to the material that caused the sensitization should be
permitted.
HAZARDOUS INGREDIENT(S):
4,4 -Diphenylmethane Diisocyanate:
ACGIH TLV 0.005 ppm (8-hour, 40 hours/week)
OSHA PEL CEILING 0.02 ppm
NIOSH PEL/TWA 0.005 ppm (10-hour, 40 hours/week)
NIOSH PEL/CEILING 0.02 ppm (10-minute)
ppm = parts per million
There is nothing "wrong" with Gorilla Glue, used for what it will do well and used with appropriate hygiene precautions. As with most chemicals, please don't get that stuff on your bare skin, as it may do unexpected and unwelcome things in the days and years to come.
From contributor Mi
I love the pic of "your hands" Jim. I used GG for a dozen or more outdoor projects using green lumber (mostly cedar). I hated that crap every minute I used it. I have since found several other products that are better for my work.
Mike
From contributor Ge
Mr. smith's comments are worth a million.
For any adhesive or chemical, Google the name of the product and then add MSDS. You will get a listing of the document that indicates risks, exposure guidelines, etc. for that product. For example, for Titebond PUR, which is a good, widely used adhesive (but is not TB 1, 2 or 3, which are pva type), try POLYURETHANE TITEBOND MSDS. The fourth entry down when I do that search has the MSDS reproduced by Rockler with all the precautions mentioned by Mr. Smith and even a bit more. In spite of the cautions, I do suggest that PUR is often the best choice when used properly.
From contributor on
I've no direct experience of GG PU, but have successfully used liquid PUs and have some background in industrial adhesives R&D.
It seems to me that the major cause of criticism of liquid PUs on wood is the requirement for tight fits and high clamping forces to prevent foaming.
Most of the failures reported seem to emanate from a lack of awareness of the need for this to avoid gaps filled by weak foam - and that these failures have led to generalised but unfounded criticism.
PU is in the wider engineering and technical world a respected structural adhesive with its own characteristics and some great properties - a respected member of the family of adhesives.
One size fits all claims haven't helped its reputation in woodworking - but are typical of most commonly used woodworking adhesives. (those targeting some structural/mission critical applications excepted)
As a user group we're not very good at differentiating between the properties of the different adhesive systems either....
PVA adhesives are a case in point. We're very used to them, they're pretty versatile and there's acres of flashy advertising material about pushing them - but has anybody here ever tried running to ground the information needed to actually design a glued joint using one?
ian
From contributor Bo
From my experience problems with Gorilla Glue are primarily created by lack of knowledge and proper procedures on the part of the user, not by the glue. We use GG for practically everything in our shop, not because it is the strongest glue on the planet but rather because it works so well.
It does have a decent learning curve and if you don't use it properly it can be problematic, much like any other glue. GG gets lots of bad press and negative comments from those who have tried it once, failed to get the results they wanted and decided it was the glues fault rather that a lack of experience or knowledge on the part of the user. We use it daily for veneering, solid wood assembly, joinery, laminating dissimilar materials, etc. So far we have had 0 failures, 0 problems and 0 reasons to not love how it performs.
Clearly there are those here who have had other experiences, just as clearly it is probably their own fault and not the glues. Just my two cents. Now if you want to talk about Unibond 800 problems I've got a stack of them to discuss. Again could be the end user that's creating the problem and that would be me in this case. To each his own I suppose.
From contributor Ro
Nothing much to add to the post concerning GG but I can empathize with Marco. I live in Mexico and I have had the pleasure of using many fine woods though often they have not been in optimal condition.
I was able to go into the jungle last year and cut dead standing Tzalam trees and, with the help of another guy, we cut them into boards using a chainsaw.
From contributor Gr
We find ourselves using loctite PL (polyurethane) construction adhesive for many applications. Does not foam, long open time, great feel while gluing up. Have even used it for veneering in a vacuum press, just squeegee it out thin.
The cons: slow cure time (no I won't spray our woodwork with water to accelerate the cure time unless its shop fixtures), and an ugly and sometimes large glue line. It is just one more tool in the toolkit, perfect at certain times.
From contributor Ke
I have done a bit of woodwork in the past but not on the level with you guys. I damaged my 12-string Guild guitar neck by forgetting my stand. The wood is high figure maple. There is a 3 inch crack now running through the middle. As getting glue in the crack was difficult, I thought GG would expand more into the crack and do a better repair than Elmer's wood glue. Boy was I wrong. In time it reacts as if I had not repaired it at all. Now I have no way to remove the GG. My question is, which glue is most likely to bond with it and the wood for a permanent repair?
From contributor Ge
First, as I stated before, there are many PUR adhesives.
At this time, you have one choice as I see it...you need to open the crack with a very small router to remove the old adhesive and form a straight sided, potentially "nice looking"repair. Then put in a wood spline that fits not too snugly and also fill the opening with epoxy. Epoxy can maintain very high strength with a large gap. (Epoxy requires a thick joint. Some of the bad reports about epoxy are because too much pressure was used, especially with a tight fitting joint, so that the joint itself was not thick enough.) Many high quality guitars and stringed instruments do use epoxy, so I suspect that the tonal properties will be ok.
From contributor Ke
I'm thinking about going ahead and using epoxy on the crack on my guitar. If that doesn't work I could alway try something more radical like using separating disk to clean out a section on each side of the crack and then using epoxy. The disk is only a mm thick, though of course the cut out will be a bit thicker. And as the crack is not completely straight the gap left will be larger in places. I've never used epoxy with wood. Can I use ordinary household type or do I need a special kind?
I can add sawdust of the right color to the outside edge to help hide it. When I use epoxy on other materials I like the stronger long setting kind and then heat it a bit with a hair dryer so it will set up quicker.
From contributor Ji
Kent,
No offense, but music instrument repair is a job best left to a professional (as evidenced by your failed Elmer's glue-up job).
First of all, the idea with any crack is to close the crack if possible. That would've involved glue-injection, clamping, refinish touch-up and a music-shop guarantee. If the crack was from internal forces and deemed not repairable or close-able, than it would've involved a pigmented filler. If the crack is structural and not repairable, than the neck would be replaced. All these variables are easily ascertained by an instrument repairman.
If this is a valued instrument, than you might consider reserving your hand-work to playing the guitar only and deliver it "as is" into the hands of a professional (before you do further damage).
If you persist with your sawdust/gorilla/epoxy over Elmer's, you will most likely fall flat.
I sorry to be so james blunt
From contributor Ke
Jim, you seemed to have missed the point of this thread - it was Gorilla Glue I used. Frankly, I think Elmers wood glue would have done a better job of holding. Now dealing with the GG, I suspect a professional would want to do a more major (and expensive) job that I can't afford. Also as I'm overseas with the U.S. military, I can't afford the expense of shipping it (weighs twice as much as any other guitar I've owned. I also have often sing during the Christmas season and really need to give it another try.
As epoxy seems to hold well with a gap, that is the glue I'm looking at. Though my experience gluing wood may not be on the par with yours, decades of professionally making and repairing both watches and jewelry have given me plenty of experience with epoxy.
From contributor Ke
A bit further of my thinking: what are the chances a luthier has dealt with this exact situation? Unless he cuts out a section and glues new wood, he may be experimenting as much as I. If we were dealing with the top or body, there would be a chance of messing up the sound of the guitar. But that is not the case with the neck. As long as it is stable we're good to go. I checked with Guild just to see what a new neck would cost and they don't have it nor would they build one.
From contributor Ke
I contacted West Systems for advise on which of their glues to use. They took enough interest to request pictures. I'm impressed! I'll let you know what they say.
I thought I might as well post them here.

From contributor Ji
Kent, I know this is post is about GG but you're asking for advise after you've already used it and made a mess. To answer your question then, there is no glue which will bond permanently with the GG and result in an adequate repair. In truth you've probably ruined the instrument (this is something which I didn't want to say).
As far as I'm aware, GG has no accepted application in the construction or repair of wood-winds or stringed instruments. The so-called "gap-filling" properties of GG is nothing more than foaming bubbles which have no structural benefits, while permanently staining and sticking to everything.
As I've said before, there are proper methods of making repairs but you've gotten off on on the wrong foot and I fear the worst.
For starters, hot hide-glue is traditional and still the best glue for repairs and construction. I could go into a long dissertation but this wouldn't undo the damage you've already done. You may as well get out your grinder and epoxy and give it your best shot. I sincerely wish you luck though and I thank you for your military service too.
As I'm sure you know, twelve-string guitars are inherently hard on guitar necks and you're not the only one who's had problems. I believe it's a common practice to leave the strings loose when not in use. This of course is no fun since you now have 12 strings to tune each time you pick it up. My own 12 string developed a bowed neck which would not come straight for either love or money. It was heartbreaking. I also had an antique zither which literately pulled itself to pieces. Now I fool around with a 3 or 4 string dulcimer.
I guess you also have guessed by now that woodworking is quite a bit different that watch or jewelery repair. Still, craftsmen like yourself will always find ways of doing good work. If it were my problem, I would probably make a whole new neck and not out of maple, which is too brittle.
Good luck.
From contributor Ji
OK I found this and other stuff...
Beautiful guitar...You need to find a way of opening the crack and injecting glue (not thick epoxy) and clamp, If you've got an internal truss rod, perhaps you might loosen it a bit and let the string-tension open the crack just enough to admit glue.
I believe however, that the problem is the figured maple which is not fibrous enough to fight all12 strings. If the truss-rod is not kept adjusted, the wood is going to fail and perhaps it will again no matter what you do. I believe I'd call this a (very pretty) design flaw.
From contributor Ke
This is the third 12-string I've owned. Before this accident it held a tune amazingly well, much better than the others. I believe this is due to the laminate down the middle of the neck. Unfortunately this same feature now prevents the crack from being opened up much. I found I could open it a little by twisting the top a bit to the side. I did clamp the joint fairly well before. From what I've read on this forum, this actually may have caused the GG to fail. West Systems makes an epoxy that is supposed to be pretty thin.
From contributor wo
The recent link points to Stewart McDonald.
As far as I know, there is no better source
for guitar related materials - they may a bit
pricey, but the cost is relative.
I would go as far to say if the glue isn't
available at StewMac, then it isn't something
you should be using for instrument repair.
Dan Ereliwine at StewMac has probably forgotten
more about guitar repair then all of us combined
will ever know - peruse their archives for
repair tips - and they have a "question" type
form at the site - who knows, maybe you'll get
lucky and get a response that will get you headed
in the right direction.
If you do, please post the results here.
As for maple being a bad species for guitar necks,
Fender has produced possibly millions of guitars
with maple necks. My experience has been that neck
behavior and longevity has a lot more to do with
the makeup of the piece of wood and the tree it
came from (old growth, quarter sawn, etc.) then
the species (from the range of acceptable species,
of course)
From contributor Ji
Yes there is a thinned-out epoxy (like water) which is for penetrating and sealing surfaces, but it's way to thin to be regarded as a structural glue. Besides as has already been said, the strength of epoxy lies in a thicker glue-line and clamping is counter-productive to that. A clamped wood glue-joint, is the best possible joint and superior to epoxy bonding.
Assembly-glue for wood instruments is usually water soluble and this allows for some dis-assembly and repair as required. It also allows for complete water clean-up which is non-negotiable. A properly joined and clamped glue-joint then, is stronger than the wood fibers and this is your goal. Don't be afraid to remove the fret board and even the neck from the body, as you're already in a desperate situation. Your only hope lies in a proper and professional glue-joint. Unfortunately, given the highly figured maple, I'd say your chances for complete success, are not particularly promising. It's definitely worth a try though, as 12 strings don't come cheap.
From contributor Ji
I agree with every word from woody...
From contributor Ke
Thanks, Woody, I appreciate learning about stewmac. I appreciate your chiming in. I notice in their teaching on truss rods that they recommend epoxy for instillation. Jim, I made two big mistakes, the biggest not preventing the accident to start with. I do appreciate your advise. But I do not believe I have ruined the guitar. Two ideas have come to me. I could cut out a good sized piece out of the middle of the top of the neck,under the the fretboard. This would leave side pieces of the maple for show. It could be a more strong and stable wood, plywood or even another material (Martin used square steel bars in some of their guitars). Or even less intrusive, steel tubing (round or square depending on the shape of the chanel) might be mounted and glued around the truss rods in the area of the crack and just on either side of it. This sounds like less work than building a new neck and would leave the guitar looking closer to original.
From contributor Ro
just thinking if u need help, maybe can ask here: www.saglumanist.com
From contributor no
AH Gorilla Glue!!!!
In the mid 90s, I was working in seattle for an outfit who did special work on special problems. One big problem in that city was water leaking through concrete foundations, walls etc.etc..
We would drill holes on a 45 degree through the wall and intersect the crack back inside the wall, We would then place an expanding port into the hole, tighten it up and inject a special "grout" under great pressure into the crack. The grout ...when mixed with the water in the leaking crack would foam ....expand ...and follow the crack as it expanded, sealing the crack entirely, If the crack was dry at the time we worked on the problem, we would inject water ahead of the grout.. about the year 2000, I came back home. One day, needing some glue, I went to the local dealer and noticed this new glue called Gorilla Glue and thought I would give it a try. I nearly fell over when i started to use it. Yeah!!! the same stuff I used 5 gallons at a time