Dowel Set-up

1/23/17       
Stewart Member

Hi Everyone,

I have searched this forum but can't seem to find what I am looking for. We are finally introducing doweling to our shop floor and are wanting to use a standard 8 x 30 mm dowel (not pre-glued). Our standard material is 19mm thick. How much of the dowel into the end bore and how much into the face? Is it better to plan on leaving a 1 or 2 mm clearance at each end of the dowel? (Or does it matter so long as there is some clearance?) Is there a standard for number of dowels in a 24" deep base and 12" deep upper? I'm thinking we have to be on 64mm centers to keep within AWI spec (?) We are planning to start the first dowel at 32mm from the face. Thanks for the help!

1/23/17       #2: Dowel Set-up ...
Bill

Based in my experience you need a 2mm gap at the bottom of the hole for the excess glue to pool. Then you need to put enough glue in the hole for it to be pushed up the sides of the dowel.

The problem is that an average assembler manually applying the glue will use less than needed so there is no squeeze out.

The answer is to get a glue application device that will apply a repeatable specific amount of glue. We use a Jolly Colla. Expensive but worth it.

You mentioned not using pre glued dowels. They work very well and are easier to have success with than glued dowels for the reasons mentioned above. You can shoot water in a hole easier and cheaper than glue.

If you are going to use a boring/insert machine water is better than glue in my opinion. If the machine stops shooting glue or water there it is not easy to tell. I suspect if you shoot glue over time you will get clogs. Then things will fail later down the line.

In the beginning we used a lamello glue bottle to apply glue. It worked well, put glue on the sides of the hole and lasted for a couple years.

I can not help you with the other questions. We overdue it.

Good luck.

1/23/17       #3: Dowel Set-up ...
Zack

When measuring for dowel outstanding the basic rule I go by is to leave at the very least 3mm of material at the bottom of your hole when you bore for your face hole. This includes the 1mm reservoir for glue. So we are talking about 12-14mm dowel outstanding for 19mm thick material. Any more then that and you will blow out the back when assembling your material.

As for pre-glued dowels they are definitely not as strong when assembling (you usually have to use PVA in the face hole anyway which means you're buying glue so why not use it for the whole dowel) and they are very temperamental to humidity and heat. *see info sheet*

As for dowel placement go with AWI standards and adjust as you see fit when in production. It will always depend on the material and application of the pieces you are making.


View higher quality, full size image (2448 X 3264)

1/23/17       #4: Dowel Set-up ...
Bill

Zack my experience tells me pre glue is sufficient. Steel dowels are stronger than wood but it turns out wood is strong enough.

The document you sited is a Gannomat marketing document not a technical document. Also glue coated dowels have been around quite a while.

If you are hand applying dowels by all means use glue. If you are using a bore insert machine I don't think it is worth it.

Either way will achieve success.

1/23/17       #5: Dowel Set-up ...
Larry

When we got our bore & insert we tested both systems. The glued dowels held better, BUT are they necessary? There aren't any problems maintaining the glue system, as long as you do it every time you use it, takes less than 5 minutes. At the clamp we use a Lamello pressure tank and gun. Again not a problem if you maintain the system correctly. At the drawer clamp we are using a Lamello bottle. Needs to be kept very clean. As for hole depth a little space is required just because there are always some variables.

1/24/17       #6: Dowel Set-up ...
Zack

Bill, I agree that wood dowels are all you need over steel. All you are looking for is shear strength in that respect and the material will break way before a wood dowel snaps.

I went to the Gannomat website to see if this was a marketing tool and it doesn't look like they are selling dowels so I believe that this is not so much a marketing tool as good information to inform the market. Many of their points look like common sense to me, especially the point about the glue on the dowel outstanding being activated thus making you have to use glue in the face hole. One of the aspects of a dowel is to soak up moister and expand in the hole to make a stronger joint which means the glue is naturally going to activate on the dowel outstanding when injected. It looks like any machine can shoot either type of dowel so why put out information in this respect against pre-glued dowels?

I have heard stories of pre-glued dowel construction being weak and coming apart and dowels jamming in the feed tubes because the already activated glue rubs onto the side of the tube making the dowels stick in more humid weather. I've also heard of groups of dowels sticking together because the dowels glue gets activated by the humid air. Another thing is that you have to shoot and excess amount of water into the hole to activate the glue properly which can run out onto your machine and rust parts.

I have never heard of these problems with normal dowels and glue. If you have a machine that can handle the glue properly and have employees that maintain the machine then a dowel with glue I believe makes for a stronger hold and better joint with less failure.

I would much rather have a 0% chance of joint failure due to dowel and a glue being properly installed then a higher % of failure using a pre-glued dowel installed properly. Are pre-glued sufficient? Most of the time yes, sometimes no. Depends on how you look at it

That's just my opinion though.

1/24/17       #7: Dowel Set-up ...
Bill

Zack the marketing is "our machine can shoot glue theirs can't". If it is on their website it is marketing.

I look at things in the long view. Over time what will I have the most success with and the least opportunity for things to go wrong.

All your points about dowels sticking together, the tube getting sticky I have not found to be a problem. The point about activating the glue on the rest of the dowel I also find to be untrue. The water is very precisely injected it is not running out the hole. It is shot at an angle so it bounces off the bottom of the hole and spreads to the sides and top. Unfortunately due to other problems we take things apart. When we do this we are in effect testing the holding force, it is adequate in my opinion.

My fear with injecting glue is that over time (think years) the system will get junked up (that's a very precise technical term). Everything we have glue in over time gets "junked up". I do not see why the boring machine would be different. Then at some point it will not shoot glue or not shoot enough glue and you will be putting product out the door that is held together by friction and it will fail 100%. If this happens it may be many many products that fail before you realize.

In my view it is just a matter of time before this happens and it is likely to happen more than once. We are very particular about our preventive maintenance. I have a full time person. I still believe that a pre-glued dowel over time is going to give me the most chance for success and protect me from mass failures.

Is it as strong as a properly glued dowel, probably not. Is it strong enough, I believe so.

We do glue the face side because it is easier to control glue than water in a hand applied application.

This is all my opinion based on experience. We have gone through 2 boring machines and so many dowels I would have to think about it to put a number on it. Certainly in the millions.

Can glue be used successfully, certainly. I would follow a strict testing and cleaning protocol.

Bill

1/24/17       #8: Dowel Set-up ...
Dave L

64 on center is for drawers. I thought doweled cases were 128, but that is for confirmats. Dowels are a more flexible 4 per foot.

I don't know the rule of thumb, but boring machines typically drill the edge holes ~11mm deeper. I prefer a minimum of 12mm face holes and 35mm dowels.


View higher quality, full size image (734 X 354)

1/25/17       #9: Dowel Set-up ...
Larry

"My fear with injecting glue is that over time (think years) the system will get junked up (that's a very precise technical term). Everything we have glue in over time gets "junked up". I do not see why the boring machine would be different. Then at some point it will not shoot glue or not shoot enough glue and you will be putting product out the door that is held together by friction and it will fail 100%. If this happens it may be many many products that fail before you realize."

There is a simple solution: PREVENTIVE MAINTENANCE. In our shop the boring machine gets its glue injection tested at every startup. It's simple, takes a couple of minutes, cheap insurance. At shut down the machine nozzle is cleaned, wiped with a light coat of oil and ready for the next day. Once a year the systems on all machines are taken apart: cleaned, lubed, checked for wear, etc. PM! This is addition to the day to day maintenance. In all the years we've run this way we've never had a call back for a joint failure.

"Unfortunately due to other problems we take things apart." Know it too well, but if you call it quality testing it sounds better.

1/26/17       #10: Dowel Set-up ...
Bill

Larry I am glad you chimed in. I believe I have read this before from you. It is part of my thinking on this subject and good insight for someone who wants to use glue.

Although we have a strong PM program the daily upkeep is not what it should be and I would be uncomfortable adopting this strategy. Lessor of the evils so to speak.

Thanks

1/26/17       #11: Dowel Set-up ...
Larry

Bill, I can understand that.
If you allow more than one user of a machine, you have to have one of them take ownership and make sure "their" machine is taken care of. I'd like to say this is 100% affective but it only works with certain people.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)