We are having a problem with plam strips adhering to particle board substraint with our edgebander. WE are getting good coverage with the glue on the particle board but are having problems with the edgebanding sticking to the glue. Before we primed the back side of the plam and that worked fine but this last job some of the edging was coming loose. Should we try coating it lightly with contact cement? We never had this issue before and maybe it was the cold temperature in the shop. We are using a holzher edgebander with cartriges. We had an scmi bander with a glue pot and pellets and never had any issue what so ever. It is also a special order laminate and I am wondering if it could be that the laminate is old. It seems a bit brittle when we route it as well. Just never had this issue before and wanted to see if anyone any ideas. Oh, buy the way there is no matching pvc edgebanding unless I wanted to have a special run made which is way more than I will ever use. We could always stick everything by hand but I that would take a lot of time.

2/12/23       #2: edgebanding Plam strips ...
MarkB

Odd… I’ve run laminate through our cartridge bander several times with no issue, I don’t trim just because the laminate is hard on the trimmer knives and I don’t want to wear a notch in them for short runs. RE your coverage are you able to see when the laminate comes loose if it’s letting go from the laminate or the core? Is the glue in several beads or is it full coverage? If it’s releasing cleanly from the laminate I would say the laminate is the issue. I wouldn’t think phenolic laminate would need to be primed like pvc does. Wonder if trying a light scuff on the back of the laminate may help but probably not.

2/12/23       #3: edgebanding Plam strips ...
d conti

It is coming loose from the phenolic back. There is complete coverage on the particle board. We had this issue in the past and a light coat of primer on the phenolic back solved the issue, but this time it did nothing. I am wondering if there could be some sort of chemical or "lubricant" that could contaminate the backside of the laminate and maybe cleaning it with some denatured alcohol would remove it and allow the proper bonding with the adhesive. We found this out when we laminated the front of the doors and during trimming the router bit would sometimes pull the strips loose at the corners. I am also going to try to increase the temperature of the glue. We have had this issue with both Formica and Wilsonart brands but both were a special order laminate, not stock colors. Both seamed to be "brittle" and not nearly as flexible as standard laminate that their stock would be turned over quite regularly.

2/12/23       #4: edgebanding Plam strips ...
Bob Lewis Member

We always prime the backside of the laminate with contact cement before slicing the laminate into strips.
Never an issue after priming.

2/12/23       #5: edgebanding Plam strips ...
Dave Edgerton  Member

Definetly have to prime with solvent based spray on contact cement. We had this issue and solved it that way.. At least 10 percent coverage with the contact cement. Let it dry, good to go. Cut the strips before you prime them otherwise you will have chips all over them.

2/13/23       #6: edgebanding Plam strips ...
Allen Chalifoux

Probably a silly question but what glue are you using?
We used to have intermittent problems with PVC and HPL. At the suggestion of a tech we switched to Dorus about 15 years ago and never had another problem.
This is on an old Brandt bander. Allen

2/13/23       #7: edgebanding Plam strips ...
D CONTI

We are using Klieberit glue. I did some research and found that some plam manufacturers use a release agent in production. Next run I will try to prime it with contact cement, that should not be an issue. Thanks for the input

2/16/23       #8: edgebanding Plam strips ...
Leo G Member

How about wiping the back of the laminate with Acetone to remove any manufacturing contaminates? Seems easier if it works.

2/16/23       #9: edgebanding Plam strips ...
Dave Edgerton  Member

@leo G. We tried that and it is hit and miss. We used formica cc spray and works great.

3/1/23       #10: edgebanding Plam strips ...
Bruce H

We prime with glue sizing. Works so far.

3/6/23       #11: edgebanding Plam strips ...
Gerry Member

We prime wood and laminate with Titebond original thinned 50% with water.

Heat will activate the glue and it sticks good.

3/26/23       #12: edgebanding Plam strips ...
Chippy1987 Member

If you don't cut the pieces before priming them, you'll have shards all over them, and prime them well and good. Agree with @BobLewis and @DaveEdgerton on this one.

4/27/23       #13: edgebanding Plam strips ...
RakeshYves Member

Edgebanding plam strips gives woodworking projects color and texture. The strips decorate furniture and cabinets by covering plywood, MDF, and particle board edges.

An iron, adhesive, or edgebander can apply the strips. The strips are available in many colors and textures to match your project. Edgebanding plam strips is an inexpensive way to finish your crafts.

5/3/24       #14: edgebanding Plam strips ...
BOB Member

Does anyone know if there is anywhere in writing that says not to bond PLAM with an edgebander? or has your hot melt person told you not to use without a primer or sizing? I'm Trying to get someone to switch to PVC instead of PLAM. I don't want to use contact.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Vacuum Pressing Systems, Inc.
      Vacuum Pressing Equipment - Including Bag and Frame Systems
    • ULTI-BOARD
      The Ultimate Spoilboard - ULTI-BOARD - Specifically Engineered and Formulated for the Ultimate in Spoilboard Performance - Not Your Ordinary Sheet of MDF.
    • Excel Dowel and Wood Products Inc.
      Plain and Pre-glued Dowel Pins, and Wood Parts - Servicing Small Hobby Shops to Large OEM's
    • Rangate
      Woodworking Machinery, Supplies and Knowledge

    Become a Sponsor today!