I'm a cabinetmaker being asked for my opinion on engineered flooring. Species will be white oak up to 12" wide. Ultra high-end job.

I've attached a photo of 3 products from 2 different vendors.

Type 1: 7mm solid oak faces with 7mm solid, cross grain core

Type 2: 4mm solid faces + 10 mm solid, cross grain core

Type 3: 4mm solid faces + 12mm Russian Birch core

My question is - The construction of Type 2&3 balance the approx. mass of solid wood with the approx mass of the core. The vendor says the ratio is about 45% solid oak (by mass) to about 55% cross band core or ply core. They argue that this provides a better balance than the construction of Type 1.

This makes sense to me but I'd like opinions. I see the appeal of the thicker wear layer which would allow more sanding and refinishing but that's not really an issue on this job.

Click the link below to download the file included with this post.

FLOORING_X3.pdf

2/2/20       #2: ENGINEERED FLOOR BALANCING ...
rescraft

Are you going to be doing the install, and the warranty that goes with it, or are you just being asked for your opinion?
I would defer to the pros that do this type of flooring, to get the word "from the horse's mouth", so to speak.
Other considerations, is this a slab on grade install, raised foundation/crawlspace? Will the home be climate controlled before/during/after the install? Just some considerations I would be thinking about.

2/2/20       #3: ENGINEERED FLOOR BALANCING ...
Orin Zelenak  Member

Website: apg10.com

I won't be liable for the warranty. However, I'm being asked to make a decision based on a technical perspective.

My opinion at this point is as follows:

1) A balanced construction means pull force of faces is equal to and countered by core.
2) Accounting for face species variations that means about 1:1 ratio of hardwood on both faces (total) to core. With a 1" board that would mean 1/4" faces and 1/2" core
3) Choice of cores between hardwood and ply may be important but are an order of magnitude less than the 1:1 ratio of faces to core.
4) Type 1 is more prone to movement than Types 2&3.

Yes or no?

2/3/20       #4: ENGINEERED FLOOR BALANCING ...
BH Davis  Member

Website: http://www.bhdavis.net

I don't like the Type 1 at all. Those 7 mm faces are strong enough to create problems with the cross grain core. At 7mm thick the faces will be trying to expand and contract along the width of the board while the 7 mm thick core is trying to do the same in the opposite direction. Based upon my experience this is a recipe for failure......especially if this is for a on slab or non-climate controlled environment.

Of the other two I'm partial to the ply core. I think that adds greater stability than the solid core. The 4 mm faces are right on the edge of perhaps trying to expand/contract on their own but probably are not strong enough to overpower the adhesive attaching them to the core, and hence, remain stable and not be likely to end up with surface cracking.

BH Davis

2/3/20       #5: ENGINEERED FLOOR BALANCING ...
Brad

I am not sure the wood flooring association guidelines permit a 7mm wear surface, but I could be wrong. A 4-5mm wear surface from Mirage can be re-sanded 4-5 times, so I don't see much benefit with the thicker option.

With 12" wide planks I would almost be leaning towards something with a built up core like Kahr's uses (see image).

You could probably reach out to Charles Peterson and ask his opinion. He wrote the book below. I have chatted with him before, and he is quite a good guy.
https://www.amazon.ca/Wood-Flooring-Complete-Installation-Finishing/dp/1561589853

2/9/20       #6: ENGINEERED FLOOR BALANCING ...
cabinetmaker

We have had the type 2 in my foyer for 21 years. Wear has been great. It is white oak veneer Lots of sports gear and luggage dropped on it over the years.

I followed the mfg’s install and added about another 1/8 around for expansion as I used to lay hardwood when younger.

It still looks good but could use a sanding. I used the mfgs cleaner and dressing as required. Never wet mopped or steamed it. That voids the warranty

It’s remained flat. My shop runs a lot of balanced panels in our work and any special veneered panels I bring in we spec balance with like species.

I have been in a few pissing matches over the years with vendors and wholesale clients that want what they want and I bill them twice when panels bow uncontrollably and peel off a wall.

I today’s market of mills pushing faster than ever for even core, proper balancing and acclimation (spread out) is imperative.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Doucet Machinery ExFactory
    Sponsors

    Become a Sponsor today!