How to make these without warping

11/15/19       
Pat Gilbert

I have to make a dozen or so of these that go into a house on the harbor.

They are alder ply (pro core and veneer core) going to be stained and lacquered at the job.

I was thinking maybe they should be sealed on the inside before assembly.

Click the link below to download the file included with this post.

Columns_2.pdf

11/15/19       #2: How to make these without warping ...
Pat Gilbert

The dimensions are 156" tall and about 30 wide by 2" at the face

11/15/19       #3: How to make these without warping ...
Ex-Pat Member

Assuming that the nosing is a piece of solid, as long as the solid is milled flat and true, you should be fine. To quote David, "Build flat, stay flat." I would certainly agree that finishing the inside won't hurt, could help. I would make sure they get assembled soon after finishing the inside though so it doesn't sit unbalanced for long. Otherwise, the only thing I can think of is to make it a torsion box with 1/4" veneered skins.

11/15/19       #4: How to make these without warping ...
TonyF

Pat Gilbert:

I don't know how much weight is saved by having strips between the two outer skins, but if you put solid material as the core and it was glued flat, there is a good chance that it would stay flat, as it would be a balanced construction with no place for environmental factors to manifest themselves against the inner face of the skins.

You could use some light weight material for the core, such as honeycomb, and groove the top, bottom, and back of the column to provide attachment to slide onto onsite blocking.

Some might argue that it is already balanced with strips as shown, and whatever happens to one side would happen to the other, with perhaps only the possibility of cupping the faces of the columns because of unbalanced finish application.

Finishing the inside first, and waiting who knows how long before the outside is finished, is asking for trouble. My two cents, I am sure others will disagree.

Hope this helps.
TonyF

11/15/19       #5: How to make these without warping ...
David R Sochar Member

If the ply panel faces are 3" thick, then you only add 1/2" strips to the interior. Space them apart about 3" or so, and you will be fine.

Your imbalance is balanced. The finish is balanced on the whole panel.

You could go to 1/2" panels and a 1" filler, and still be balanced. At 1/4" panel faces, I would then go to an egg crate of a sort, and a full on torsion box.

Use a more rigid glue rather than a less rigid (TB2 or TB3).

And "Build flat, stay flat" is wise. Make a solid structure that these can 'pile' onto as they are assembled. Be sure it is very flat, and all panels are oriented the same way.

Design-wise, I hope these are far enough apart that one can't sight one against the other, or slight differences in 'flat' may be apparent. At 2" thick and 13' tall, they could act like a piece of paper stood on end.

11/15/19       #6: How to make these without warping ...
Adam

Use 3/4 x 2 solid jointed straight for the nose. The nosing and the fixing to the wall will keep it straight.

We typically use a bit of glue and a cabinet stapler for the blocking. Be careful to lay the big panel down on a flat table. Clamp the whole thing to the flat table not saw horses when putting the 2nd piece of ply down. Otherwise you will induce a bow.

11/16/19       #7: How to make these without warping ...
Karl E Brogger  Member

Website: http://www.sogncabinets.com

If you REALLY want to go over the top....

It won't move


View higher quality, full size image (3024 X 3024)


View higher quality, full size image (3024 X 3024)

11/16/19       #8: How to make these without warping ...
Pat Gilbert

Thanks for the input, very useful

Karl is that lattice necessary for a torsion box?

11/16/19       #9: How to make these without warping ...
Karl E Brogger  Member

Website: http://www.sogncabinets.com

Sorta. It was basically a subframe for a stainless countertop a buddy was making. It was supported all the way, so it was more just for filler. It probably didn't need to be at an angle, but the steel was going to be longer than we had material for, so making it like that was an easy way to make it longer than that material available. I was also screwing around a bit. When you're not making any money anyways, might as well experiment.

It wasn't super stiff on it's own, but sheeted and properly adhered, I'd bet it would be bonkers stiff.

For what you're doing, I'd just run some dados to index placement of the strips like David said. For me, I'd probably glue them up a little oversized, then trim them to size on the panel saw just to make sure the two edges are perfectly planing out. My panel saw only has a cutting depth of 2¼ though, so if thicker than that, I'd have to re think my approach. Then just apply the face edging.

Or.... I don't have enough length on my cnc, and you wouldn't get that out of a 5x12 anyways, but a big miter fold like that looks pretty sweet and seamless.

11/16/19       #10: How to make these without warping ...
Pat Gilbert

I'm not sure that these the filler strips at all

These are going to be screwed between cabinets in spots

11/16/19       #11: How to make these without warping ...
Pat Gilbert

these the filler strips at all = the filler strips are needed at all


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Lamello