Subject: Re: Dry Mil Thickness Calculations?

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Dry Mil Thickness Calculations?

11/14/18       
DanShaf Member

Magnalac has at most 30% solids by weight and also 24% solids by volume. If I spray 3 applications, each of them 4 - 5 wet mils, will I achieve 3.9 - 4.5 dry mils or will I achieve 2.88 - 3.6 dry mils? That is to say, to do the math on my dry mils should I be using the percentage of solids by weight or by volume.

11/14/18       #3: Dry Mil Thickness Calculations? ...
nick

My guess is the later,,,with a wet film gauge you're measuring volume not weight,

11/15/18       #4: Dry Mil Thickness Calculations? ...
JM

Use volume for your calculations. Weight doesnt matter for the intended use. Mfg put weight on as it shows a higher percentage so looks better....marketing crap.

Also dont forget when you scuff sand between coats, you are removing some material, so you will be less than calculated.

11/15/18       #5: Dry Mil Thickness Calculations? ...
Collin Parker  Member

Website: heritagewoodwright.com

your numbers looks funny. should be .24*(4 or 5)= .96 or 1.2.

dry mil= wet mil * %solidsvolume

11/15/18       #6: Dry Mil Thickness Calculations? ...
Brian Member

The coating manufacturer should be able to run a dry mil check for you on a finished panel if you are trying to determine if you are applying their system to the correct millage. Check with your distributor.

11/15/18       #7: Dry Mil Thickness Calculations? ...
DanShaf Member

Collin, then multiply that by 3 applications. Not how much per application. 3 applications, each one 4 - 5 wet mils.

The percent of solids by weight is important for EPA considerations, i.e., what is the weight of the material that you are expelling into the air. If a shop is a large quantity generator, they want paperwork filled out by you so they can see on paper the amount of waste that you might generate. But I'm not asking any EPA questions or VOC questions, only questions of calculating total dry mils.

Measuring it after the fact isn't what I'm after. Only the math because when I'm deciding on a finish schedule to play with, I need the details. That would include if I plan to do a washcoat, anywhere from 3% - 12% solids depending on the amount of sizing I want to introduce into my finish schedule.

11/16/18       #8: Dry Mil Thickness Calculations? ...
Shane

Buy a positester from gaurdo and be done..... that is the only true way to know....

11/16/18       #9: Dry Mil Thickness Calculations? ...
DanShaf Member

A testing tool will measure the thickness of the coating but it does not tell me whether to make my calculations using the solids as a percentage of volume or to make my calculations as a percentage of weight.

My inclination is this, we mix up a quart of finish without regard to weight. We know that one quart of water weighs 32 ounces. We are not mixing water. In most cases a quart of finish will weigh in at more than 32 ounces, yet it will still only be one quart of that material.

The question arose at work, volume versus weight. We aren't looking to measure what we are laying down, we are looking to calculate it properly in the first place.

11/16/18       #10: Dry Mil Thickness Calculations? ...
Collin Parker  Member

Website: heritagewoodwright.com

Sorry about that Dan, didn't realize you did the multiple coat X. Anyways, I've actually switched to making my spreadsheet for paint needed per sqft based upon tested values AFTER reduction etc. You can attempt calculating based upon the % solids, % efficiency of spray equipment, % reduction... but its all a crapshoot. Time tests on multiple jobs is much better in my opinion. Just track how much raw paint you use and divide by sqft and get yourself a baseline to move forward with. Only takes a couple jobs to get decent numbers for all of your frequently used primers, stains, basecoats, clears. KISS (keep it simple stupid) p.s. not calling you stupid haha

11/21/18       #11: Dry Mil Thickness Calculations? ...
Mike Holt

To calculate your mill thickness, you use volume solids. Using round numbers, if you have a 25% volume solids finish, that means 75% of the material are solvents that will evaporate as it is sprayed, drys and cures. If you put down 1 coat that is 4 mills
wet, it will dry to 1 mill because 75% is solvent that will evaporate. To get a 4 mill dry film you would need 5 coats if you are sanding between coats.(because you remove material with sanding) 4 coats if you don't sand. To figure coverage - if you had a finish that was 100% solids and you applied it 1 mill thick it would cover 1644sq ft. So if your finish is 25% volume solids it will cover 25% of 1644 sq ft. in 1 coat.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)