Total Finishing Supplies

Professional Finishing

You are not logged in. [ Login ] Why log in
(NOTE: Login is not required to post)

Post a Response
The staff at WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at any WOODWEB Forum. Participants should undertake the use of machinery, materials and methods discussed after considerate evaluation, and at their own risk.
Your Name:
Your Website:
Email Address:
Subject: Re: vinyl sealer adhesion

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

vinyl sealer adhesion

1/25/20       
pascal stgelais

Hello everyone.

I have adhesion issue using vinyl sealer.

The wood is bare ash( no refinishing) I sand it to no more than 120 grit since at 150 I get seem to have issues.

The schedule:

-dye
-washcoat(3% vinyl and applied WET since dry coats seems to cause trouble)
- sand with 150 grit(yes 150 since 220 or 320 as recomended by manufacturer cause the next vinyl coat to just lay on top of the stain)
-oil wiping stain
- toner( dye with 3% vinyl one light coat)
-no sand toner
-vinyl wet coat
-CV

1rst question concerns first the wood. I have seen various people recommanding to sand no more than 120. I have also tried raising the grain with before the washcoat to get more grip before the washcoat.

2nd concerns toner should i scuff that coat.and is it ok to make it with viny since my CV dont like thinning

3rd I have been able to get good results so far but always end up with a more fragile finish when staining than barewood selfseal. is it normal(the result is still pretty hard though)

1/25/20       #2: vinyl sealer adhesion ...
Jim Clark  Member

That oil stain can be a problem if it's not
thoroughly dry.
I give it several days myself.
I sand everything to 220 grit and
spray wet. Haven't had any problems yet.
I do thin my sealer 50%, which is a lot but
it lays better and gets in the wood better.

1/25/20       #3: vinyl sealer adhesion ...
pascal stgelais

Regarding the stain it is supposed to be able to be topcoated after 1 hour (mohawk) although i prefer to wait until I cant smell the mineral spirit/paint thinner sent.

when it is dry do you scuff sand the stain?

regarding vinyl sealer the pds sheet state no build limits other than the total system but I suspect that building it too much is the problem because to rule out stain I applied cv directly over the stain after like 30 min when it still smelled oil and no failure.

I used to Dye-washcoat-stain-vinyl seal-vinyl toner-vinyl seal and by the last vinyl seal coat it became very fragile. Or if it seems good as soon as the first coat of cv gets sprayed the finish gets brittle

Even if the manufacturer give no limit when reading similar products from other brands most state a 0.5 to 1mil MAX thickness.

so regarding the vinyl am I right trying to apply as less as possible.

If I try the following schedule :

dye
washcoat vinyl 3% solid
sand
wiping stain
sand or no sand ?
vinyl toner 3% solid
sand or no sand?

normaly here I applied a full solid coat of vinyl but it always ended up fragile. should I just go with CV after the toners. this woild result in just 2 coats of vinyl sealer 3% wich would result in a minimal build

1/26/20       #4: vinyl sealer adhesion ...
mastercabman

Your schedule sounds complicated!

1/26/20       #5: vinyl sealer adhesion ...
pascal stgelais

I know thats why I am trying to simplify it as much as possible. I will try to put thw toner color directly into the topcoat wich will eliminate a step and thus reduce overall build

-dye
-vinyl washcoat 3% solid*
-sand
wiping stain
-CV (tinted with transtint dye)

*although my ash doesnt really blotch this step help bind the dye because if I apply the stain and wipe it directly over the dye I end up removing some of the dye.

the 3 color steps is the only way I get statisfying results because neither alone seems to do it

1/26/20       #6: vinyl sealer adhesion ...
cabinetmaker

Are you catalyzing the vinyl ? And, why the dye over the oil ?

1/26/20       #7: vinyl sealer adhesion ...
pascal stgelais

the wood is dyed FIRST
then washcoat
then oil wiping stain

the vinyl is not catalyzed since the manufacturer told me strictly to not catalyse the vinyl even with catalysed finishes. They manufacture no catalysis for it and trying to catalyse it with any product would be detrimental.

I am now trying different grits when sanding the vinyl sealers because sanding it with 220 as they recommand might not be coarse enough. I will try 150-180-220 on a test board

1/26/20       #8: vinyl sealer adhesion ...
Leo G Member

Unless you are experiencing blotchy staining why are you applying a vinyl coat between the dye and the stain. Unless they are the same resin base the stain shouldn't move the dye around (melt it).

So it should be dye, stain, vinyl sealer no thinning (catalyzed if using a catalyzed topcoat) scuff, topcoat, scuff, topcoat done.

1/26/20       #9: vinyl sealer adhesion ...
pascal stgelais

thanks for your answer leo

I am currently testing your schedule but wil change the EZ vinyl sealer for a conversion sealer( both mohawk).

maybe the problem is there. I have asked the question to 2 diff. person at mohawk ( 2 phone 1 email) and they all confirmed that this vinyl sealer MUST NOT be catalysed even under precat/postcat/CV. No catalysis exist for their vinyl sealer.

anyways this vinyl sealer as always been problemating since it always ended up brittle and easy to scratch/flake whether I sprayed it wet/dry/unthinned/thinned. Somehow sometime I was able to endup with a hard vinyl coat.

anyway as stated I will be receiving mohawk conversion sealer and will try it. It will then be a catalyzed sealer topcoated with catalysed topcoat. So my routine will be:

dye
oil wiping stain
conversion sealer
sand
CV mixed with transtint dye (as general toner)

I will probably put mohawk reducer retarder 5% in sealer/topcoat since my ash seems to bubble a lot.

1/29/20       #10: vinyl sealer adhesion ...
Matt

You may be applying the stain too heavily. This is the only thing I've encountered in my finishing life (since 2004) that predictably can cause adhesion issues.

I suggest you skip the vinyl sealer altogether and just use a good stain and conversion varnish.

If the stain isn't coming out dark enough, wipe the surface of your product with a wet rag just enough to raise the grain (make it fuzzy). Let the water dry off and then stain your product. The stain will end up MUCH darker and much less blotchy.

Don't use an oil stain for this. Use a common industrial alkyd resin stain.

Let the stain dry for a good 2 hours and follow it with 3 full coats of conversion varnish. No sanding sealer, no vinyl sealer needed.

Scuff sanding the first coat of conversion varnish will be a bit tedious if you used water to raise the grain but the second coat will sand as flat as glass if you have good sandpaper.

As long as you're using a good quality conversion varnish, self-sealing is usually going to adhere better.

1/31/20       #11: vinyl sealer adhesion ...
pascal stgelais

I have solved my problem. at least partially.

I have ordered mohawk conversion sealer. I have tried 2 schedule :

-dye
-wiping stain
-conversion sealer
-conversion varnish tinted with dye

-dye
-wiping stain
-vinyl toner (thinned to about 3% solid)
-conversion sealer
-conversion varnish(untinted)

now regarding resistance the first one seem to have an edge over the second but the second one yield better results.

I think I was applying too thick of a wet coat. I bough a glass piece and mesured my wet coat on it since it doesnt absord the liquid.

I ended up spraying almost 3 4 semi-dry pass to get a good wet coat and avoid spraying too thick

10/4/21       #12: vinyl sealer adhesion ...
LillianShar

When we apply the new material, it kind of repeats the contour and geometry of the old material. Or the wood itself, as in your case. Therefore, it's essential that when sanding, the surface is free of defects. This is why you need to smooth the surface to 120 grit. You can read more about Seal With Ease; maybe some sealers work well with 150. I don't have one of those.
For one thing, I don't apply them. It's mostly more to MDF surfaces. On hardwoods, that kind of sealant doesn't work. In any case, the adhesive needs to be applied to a clean, degreased, but not wet surface.

Seal With Ease

3/21/22       #13: vinyl sealer adhesion ...
jizzy

It all depends upon the quality of the wood you are going to use mate!

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!