BAC Sherwin-Williams Wiping Stain

3/30/20       
Mike Member

Hello group! I have a problem and I'm hoping for the right answer since I trusted my dealer and stained the entire project.
I'm using a Sherwin Williams BAC black wiping stain on white oak. I applied one coat but it was so light after wiping it off I then applied a second and third coat without wiping it off in a good continuous wiping method so that it looks perfect.
This stain is dry but if I run my finger over the product my finger will pick up a very, very tiny amount of stain and it does feel a tiny bit damp. I called Sherwin Williams tech support and he told me that the pigments did not penetrate the wood and if I proceed to put on the T65F520 sanding sealer and finish with the T65F550 that he's worried that the finish will pull off in sheets at an undetermined later date because the un-penetrated stain will act as a barrier. So my question is, is this true? Should I continue waiting until it's completely dry and then finish? The stain on the white oak looks beautiful and it does look like it penetrated. I should also say that since I have been staining the white oak it has been raining for close to four days now and the dampness in the atmosphere maybe holding the drying back. Anyway, what does this group think?

Thank you!

3/30/20       #2: BAC Sherwin-Williams Wiping Stain ...
Josh Koschak

Let it dry a couple more days and you should be fine as long as you weren't just lightly wiping it down (i.e. trying to paint the color on).

After this, switch to MLC wiping stains. You can achieve dark rich color without the headaches of BAC and MLC dries so nicely. I would never go back after I made the switch.

3/30/20       #3: BAC Sherwin-Williams Wiping Stain ...
Nick

I think that there's very little binder in BAC stain. In other words it's mostly thinner, a little pigment and color there not much holding the pigment & color together after the thinner evaporates. That's why it's coming off onto your hand not that it isn't dry. I can see there being top coat adhesion issues if lay on multiple coats without wiping.
I use quite bit BAC stain and l've found if l need to get a deep color. I dye the parts close to my stain color first before staining.

3/30/20       #4: BAC Sherwin-Williams Wiping Stain ...
rich c.

First I'd let that project sit and experiment on scrap like you should have done in the first place. Why guys experiment with a new product in their shop, directly on completed work, I'll never understand. If it was me, I'd wash off that surface, let it dry throughly. Then apply dye to get the color intensity you want, let that dry. Then clear coat. Even if you don't get an adhesion issue with what you have, that first clear coat is going to pick up that pigment and you'll have a good chance of having a muddy finish. So recreate your current work on scrap, then do the experiments from there!

3/31/20       #5: BAC Sherwin-Williams Wiping Stain ...
Mike Member

Thanks group for your responses. I like josh's response and I think it will work. I did a test piece (I know) and finished with the sanding sealer and finish and did not get a muddy pick up so I'm tempted to move forward. Rich has the idea that I was thinking and that is to wash it all off and get some General Finishes die and start over since there is a lot of time with this pandemic going on. Every once in a while no matter how old I get I still make stupid mistakes and I thank the good Lord above that I have a great group like this one to lean on!!! I'll let you know my decision. Thanks again!

3/31/20       #6: BAC Sherwin-Williams Wiping Stain ...
Dan Cook

your always better on darker finishes to start out with a dye and then follow with a stain. You don't get the muddy appearance and adhesion issues and you can still see the grain coming through. If it still isn't dark enough you can mix up a shader with the dye and darken even further.

3/31/20       #7: BAC Sherwin-Williams Wiping Stain ...
Anthony J. Darbenzio  Member

I completely agree with Josh.
While S.W. & M.L.C. are owned by the same
company, their finishes are different.
I switched 10 years ago. Best thing I ever did. When you deal with M.L.C., your'e
dealing with professionals.

3/31/20       #8: BAC Sherwin-Williams Wiping Stain ...
Dan Cook

Not sure what all of you are finding but the price of MLC here has gotten so far out of control that we switched to Sherwin Williams. The price is literally less than half of what I was paying for MLC. Maybe its the local supplier but that is just too much difference. I have used MLC for 20 years + and they just got too expensive for their products!

3/31/20       #9: BAC Sherwin-Williams Wiping Stain ...
MarkB Member

We have the same issue as Dan with MLC though they were our best option in the area when available for color match and product support. That said, we are in a pretty low volume area and MLC simply will not support a low volume area or allow you to get access to samples or less than case quantities. Its a major nightmare for a small/varied shop especially if you spray water clears. This has all come to an end in our area as for the second time in perhaps 5 years MLC has lost its distribution in the area (local distributor dropped the line due to volume) so now, if MLC will even allow it, your left paying freight to ship product in and given the stuff is already priced like gold bars thats a major deal breaker.

We are in the process now of setting back up with Sherwin Industrial (which still has to be shipped in but the base material cost is far more reasonable). We ran BAC for a long while and I would agree that MLC's spray and wipe is really nice but it is what it is.

My experience is the same as others with BAC, no binder, it will never lock up on the work (which is kinda nice when you find an errant rag mark or other issue with the stain in the booth you can correct). MLC is not so forgiving in that area for us in that going after a stain issue usually leaves a light blotch. But the BAC, for me at least, is a lot harder to work with. I dont really know how you could do much a build up with multiple coats of BAC as in my experience your end result gets lighter and lighter because you just pulling off the unbound pigment with each successive application unless your spraying it on and then your back to the thick/adhesion issues.

4/1/20       #10: BAC Sherwin-Williams Wiping Stain ...
Mike Member

MarkB, what are you saying? Should I wipe the BAC stain off or do you think the sanding sealer and finish will hold on?

4/1/20       #11: BAC Sherwin-Williams Wiping Stain ...
rich c.

Dan Cook, You've lost bids because the finish is too expensive? I've always found that no matter what finish I use, it's a tiny fraction of the cost of the job.

4/1/20       #12: BAC Sherwin-Williams Wiping Stain ...
MarkB Member

Was pretty much saying that in my experience with BAC (if your wiping/ragging/brushing) it on, I dont really know how you can build up multiple coats because for us the next coat re-wets the last and you wind up pulling more stain off than you are putting on and it seems to devolve from there. If you have it on super thick, or were spraying, I would think there would be a good risk that the stain will be a barrier and you may have adhesion issues but we spray water so the comments to let it dry thoroughly and go on may be sound.

Other than spraying I've had pretty much zero success with either BAC or MLC spray and wipe. I wouldnt say I would never see some pigment on my finger if I wiped after applying but if your seeing what you feel is a decent amount of pigment on your finger after a day of dry time I'd be concerned. I spray clear on MLC and BAC regularly in 30-40 minutes and have never had a problem though many here state days of dry time. The reason I use them is because of the super fast dry time.

4/1/20       #13: BAC Sherwin-Williams Wiping Stain ...
MarkB Member

** Correcton ** Other than spraying to build up multiple coats, Ive had zero success building up BAC or MLC. Both are great, I find MLC easier, but its a one and done deal. We rarely even let it sit for a while before ragging off because you start pushing it around and it seems more work than getting it right from the start.

4/1/20       #14: BAC Sherwin-Williams Wiping Stain ...
Mike Member

I decided tomorrow I'm going to start wiping everything off with acetone and let it sit
and let it evaporate for a few days and then apply a new stain. I won't be able to get all of the BAC stain out and they'll be a small amount of color left behind. Today I purchased General Finishes black water-based stain. So my question, do you think I will have some kind of chemical reaction with the old BAC stain left in the white oak along with wiping it down with acetone and finishing with General finishes water-based stain?

Thank you!

4/3/20       #15: BAC Sherwin-Williams Wiping Stain ...
MarkB Member

No

4/4/20       #16: BAC Sherwin-Williams Wiping Stain ...
Mike Member

I stripped the project of the BAC stain with lacquer thinner the other day and allowed to evaporate. Today I applied two coats of General Finishes black water-based stain.
The project looks great and the stain is going to stay for good and is solid as a rock.
I'll inspect the project to see if there's any blonde White Oak flashing through and if so i'll apply a very thin light coat of the General Finishes black stain. I feel very relieved that I stripped the BAC stain off and starting fresh. Tuesday i'll start finishing with clear coats.

4/8/20       #17: BAC Sherwin-Williams Wiping Stain ...
John Member

That was the right choice Mike. I didn't wipe BAC wiping stain well enough on white oak in an attempt to get a really deep color. I had the same issue with it pulling off on my finger even though it dried in less than 30 minutes. I sealed and topcoated it and all was and is fine except it chips pretty easily so there's no real bond between the finish and wood. Thankfully, it was a personal project so no harm done.

I still like and use BAC wiping stain because it's local and I can get them to custom mix it while I wait and adjust it until I'm satisfied. I've spent nearly an hour there a couple of times and they didn't complain about the time for a $25 sale. But for really dark colors I dye it first now, as others suggested, and then follow up with BAC.

John

4/10/20       #18: BAC Sherwin-Williams Wiping Stain ...
mauricio poli

I do not like to use this kind of Wiping Stain direct on the wood because of it. If you want a dark color, no way, you will never get it. So I do prefer the old NGR stain in the spray gun, applying until near the final color, and before the final top coat again another coat of NGR just to match all the pieces. If I want more contrast I make the NGR slower and apply more wet.

3/12/25       #19: BAC Sherwin-Williams Wiping Stain ...
Melissa

Help!
I used the BAC wiping stain on the bottom step of our stairs, (carpeted stairs & wood bottom step)…horrible idea, I know.
After it had dried for only 8 hrs, my daughter stepped on it.
I tried to fix it…get the foot smear off, and the stain looks way worse now.
After reading reviews, I see that this stuff can be a nightmare.
How soon can I start over? Do I sand it? I was going to get some MLC stain that has been mentioned.
Any thoughts/advice are greatly appreciated!!!


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!