Vinyl Primer taking to long to dry

4/14/22       
scott

Shooting a Chem craft CV finish bright yellow. We were supplied a clear vinyl sealer tinted yellow and after priming with it using correct % catalyst it is taking about 4 times the amount to dry. Technician claims its the tint that's causing it to take so long to dry, about 30 hours before we can sand without balling up. Any thoughts??

4/14/22       #2: Vinyl Primer taking to long to dry ...
Bob Niemeyer  Member

Website: niemeyerrestoration.com

My question to the Rep would be what type of colorant was used and at what percentage.

4/14/22       #3: Vinyl Primer taking to long to dry ...
RichC

A local shop tinted it?

4/15/22       #4: Vinyl Primer taking to long to dry ...
scott

This is same company that has tinted our colors for ML Campbell for 20 years, they now have switched to ChemCraft. They have tinted both pigmented and clear finishes in past with no issues.
My finisher logs all materials mixed and % of each. Not a problem of missing catalyst.

4/15/22       #5: Vinyl Primer taking to long to dry ...
Chemmy  Member

Do they tint all types of their finishes.? It is easy to add the wrong pigments or dyes if many types are being used.! It may be a case of using a pigment not compatible with the Vinyl, but was the right color for the tint, there are many yellows as you know. That said I would ask the name and type and company that supplies them, and go directly to that company and find out for sure if that individual yellow is compatible with Vynil your using or not.! Give them the MSDS on your product if necessary and the brand name of the vinyll.! Vynil is known as polyvinyl chloride which should be listed as the main constituent in the MSDS .!

4/16/22       #6: Vinyl Primer taking to long to dry ...
Quicktrim

We switched recently when Louis and co went to chemcraft from ml.

They sold me the select line of precat sealers and primers and it was a nightmare to use and sand .

Afterwords they admitted it only works if you have a cook off oven to cure it .

This after selling me 1000's of dollars of tinted primers that they wouldn't take back .

So I went to Sherwin Williams and their products from the west Evans branch have been very good .

Now the rep is calling asking to give me some credit to get my business back .

I say refund it all as it has cost me countless hours of rework and wasted time .

4/16/22       #7: Vinyl Primer taking to long to dry ...
Chemmy  Member

Boy...I hear you loud and clear on this matter
Quicktrim.!!
It's a crying shame that the small business man has to suffer the consequences of a middleman selling product that they don't inform the purchaser of all of the necessary info upfront of how to properly use there products being sold and
The does and don'ts or must have's about the product(s) being purchased.
The large companies being supplied with materials always has a performance guarantee
They sign between the coatings company and the end user which covers any losses incurred in use of their products, including all loss of time, not only in the finishing, but the remaking of the goods, and overtime to keep their schedules on track.!!
We had such at OSF with SW back in the mid nineties, as well as others. They were also obligated to provide a technical chemist, to both train and troubleshoot any and all problems 24/7
As we were running a two 12 hour shift around the clock 6 days a week, and 1 shift on sundays.!
Unfortunately, small companies will never get that type of deal, you have to be buying millions of dollars worth of product to do so.! And the coatings Mfg. Has to be big enough to both absorb any losses that occur without going bankrupt.!
Just know there have been may small shops that have suffered this problem including my first business back in 1970 in Florida. It hurt me bad at the time.!

4/20/22       #8: Vinyl Primer taking to long to dry ...
Adam

I have used chemcraft for 4 years now, I have Never used a vinyl primer they have specific primers for post cat and pre cat, you only use vinyl sealer when you are using clear. I Will say that I have used about every line out there over the years, and I have found that chemcraft is far an away superior My guess is you're using the wrong product, they vinyl sealer they provide doesn't get catalyzed, the primer does, I don't have access to the part number, but it should powder sand in an hour or so, pre cat, 30 minutes.

4/23/22       #9: Vinyl Primer taking to long to dry ...
cabinetmaker

Chemcraft ?

Someone screwed up

We have shot a lot of Chemcraft and this never happened Course I banned vinyl sealer of all sorts from our shop years ago

12/12/22       #10: Vinyl Primer taking to long to dry ...
Jon W Member

Vinyl Sealers are typically low solids off the bat, like 17%ish. Any more than around an oz per gallon and you are going to have problems with drying and softness of the coating. Need to make sure you are using a high solids vinyl sealer if tinting and also, remember that most vinyl sealer are meant to be sprayed on thin. If you are putting on thick layers if vinyl like you would a primer then this may be causing problems too. Chemcraft makes a white vinyl primer that you can add a bit of yellow to and also it can be catalyzed at 3% to speed up curing and enhance hardness as well as compatibility with post cats and CVs.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs

    Become a Sponsor today!