Sideboard - solid wood or plywood construction?

4/23/15       
Rsukra Member

I have a commercial client who will be commissioning 18 sideboards (or credenzas), approximately 7'L x 29" H x 25"D. They will be freestanding pieces of furniture, not cabinets, and will contain one AV rack in a center bay. 3 sliding doors. This is an office situation in New York City and the sideboards will be situated in conference rooms.

The client's preference is a for a solid wood carcass, something I have a lot of experience doing, but only as one-off custom pieces of furniture. I tried explaining the benefits of a sheet good in this case, and I've been asked to provide a quote on the difference in price.

The benefits of plywood I see in this case are:
-Avoids a serious amount of milling for 18 cases, plus the waste by-product. I've calculated it would be 4000 linear feet of panels at 25" wide.
-The fact that I only have a 20" W planer, and the case depth is 25"W
-Simplified case joinery
-Overall speed
-No concerns of wood movement

Cons: durability and aesthetics (considering that the client wants the 'look' of solid wood)

How would others alter their price? 30% more for solid wood? Are there any other differences between the two options that I'm not factoring in?

By the way, doors will be shop-veneered panels. I entertained the possibility of veneering the cases myself with 1/16"T veneer, but that might be as much work as starting with solid from the beginning.

4/23/15       #2: Sideboard - solid wood or plywood c ...
rich c.

Source out the solid panels. Then you know the exact pricing and don't have to worry about machinery.

4/24/15       #3: Sideboard - solid wood or plywood c ...
markbattles Member

Website: http://v-dubfurniture.com

Plywood is a sheet material manufactured from thin layers or "plies" of wood veneer that are glued together with adjacent layers having their wood grain rotated up to 90 degrees to one another.

4/24/15       #4: Sideboard - solid wood or plywood c ...
D Brown

Perhaps you could design a frame and panel ends with solid or veneer panels ?

4/25/15       #5: Sideboard - solid wood or plywood c ...
Nick Christensen Member

Website: http://www.littlesaplingtoys.com

I would say you need to try to better educate your client, I have run into this a few times. People will often consider veneered sheet goods to be solid wood. They think that plywood means melamine or something similar. You may be thinking of the same thing and using different terms for it. Tell them that you will use solid wood if they want to pay for you coming back to fix it every year for the next 20 years or they could have the same look with durability of plywood at a third the cost.

4/27/15       #6: Sideboard - solid wood or plywood c ...
Rsukra Member

Thanks for your input guys. Unfortunately frame and panel isn't an option because the client wants a very modern look. I hadn't thought about shopping out the milling but will look into that, just not sure who to contact in the area.

I have a feeling that they're going to want to go for solid wood in the end, I'm mainly trying to figure out how differently to price the two options. It's a tough calculation to make and the sheer volume of the pieces makes me a little anxious.

4/28/15       #7: Sideboard - solid wood or plywood c ...
Snaglpuss

Why not consider veneered mdf sheet stock and not plywood.
The mdf almost alway will look flatter and smoother, no ripples and core telegraph.
There is a reason almost all arch. millwork casework is made with sheet goods.

4/30/15       #8: Sideboard - solid wood or plywood c ...
Peter Petersen  Member

Website: http://signalement.com/home.php

I would suggest you plywood construction. Plywood is a sheet material manufactured from thin layers or "plies" of wood veneer that are glued together with adjacent layers having their wood grain rotated up to 90 degrees to one another.

http://signalement.com/

5/4/15       #9: Sideboard - solid wood or plywood c ...
B.H. Davis Member

I wouldn't make a solid 25" deep cabinet side wall. The only prayer of something like that not moving to the point of failing is if an extremely stable 1/4-sawn material were used......and even then I'd think you could see failure at that depth.

On the other hand an enclosed city office environment is working in your favor. That space will likely be much more climate controlled than in a residential installation. Even so I'd be looking for something that gave the look and feel of solid without the chance of failure.

I don't think 1/16" thick veneer on a panel base is going to be the solution either. 1/16" thick material is thick enough to have it's own way with expansion and contraction. 1/128" thick veneer is sized that way not only for cost cutting but also for stability.

I once did a series of hard maple CNC photo carvings on approx. 9" x 12" material. These ended up about 1/8" to 3/16" thick at the picture frame edges and about 1/16" to 3/32" thick in the carved field. They were then glued to a 3/4" MDF backer which was painted black on the edges and back.

Any of these plaques that went into northern non-humidified heated space had the "veneer" overpower and split the MDF, with the maple carving curling up from the top and bottom. Those that went to humid locations such as Florida are still fine to this day. While hard maple was a poor choice with regard to stability (but the ideal photo carving material) this was a real lesson in the strength of wood.

BH Davis

9/9/19       #10: Sideboard - solid wood or plywood c ...
Coastal Chic  Member

Website: casagoda.com

I have come across a situation like this just this week and still have to get back to the customer with a quote. Which solution did you go for in the end?

9/29/20       #11: Sideboard - solid wood or plywood c ...
auraadesign  Member

Website: https://www.auraadesign.co.uk/

You understand the materials and your work very well. You must communicate this information and knowledge very clearly to your clients. Plywood is a material that is manufactured from thin layers or piles of wood veneer that are glued together. It is an engineered wood from the family of manufactured boards that include medium-density fibreboard and particle board.

Plywood might prove to be more expensive compared to other options of materials that you consider. There are several sizes and finishes available and can be used for finish work, it also doesn’t get swollen from water or moisture, it can also be used for beneath flooring and will no longer contain formaldehyde in 2019.

There are certain cons as well as it is more expensive compared to other materials and options presented, it is also not as environmentally friendly as those other options, again it is not so potentially durable compared to those options, and the panels are also not as large compared to other panels.

Appearance wise plywood can offer various styles and appearances and made this way designed for building cabinets, shelves, and other items. It may have knots or a rough surface and this plywood is used beneath the finished material. For the better result you may choose any as per your client’s requirement. Also if you want to make interior space more appealing then you may set up a round meeting table and chairs and create the best environment for a conference room.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Shop Gear Inc.
      Distributor of Co-matic Power Feeders, Le-matic Portable Edgebanders, and Supplier of Woodworking Machinery, Tooling and Accessories in North America
    • Vexor Custom Woodworking Tools, Inc.
      Custom and Standard Router Bits, Shaper Cutters, Profile Knives, Multi Profile Insert Tooling and More
    • Veneer Systems Inc.
      Specializing in Veneer Equipment and Veneer Supplies
    • Rangate
      Woodworking Machinery, Supplies and Knowledge

    Become a Sponsor today!