Sawing and Drying

You are not logged in. [ Login ] Why log in
(NOTE: Login is not required to post)

Post a Response
The staff at WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at any WOODWEB Forum. Participants should undertake the use of machinery, materials and methods discussed after considerate evaluation, and at their own risk.
Your Name:
Your Website:
Email Address:
Subject:

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Sawing timbers for maximum strength/grade

4/6/20       
Carl

I have a project coming up where I'll be sawing
white ash logs into 5" X 8" x 14' to 16' timbers for
use in timber frame trusses of sorts - the loading
will be the same as roof rafters. The unsupported
span is in the neighborhood of 10 feet.

My question has to do with pith located in
the timber. I have a number of straight tree stems
that could easily produce one 5 X 8, and some that
could produce two 5 X 8 timbers, and I'm looking
for input on how the location of the pith effects
the strength/grade of the member.

I'm familiar with the basic grading rules for
structural timbers (from FPL tech notes), and it
appears that pith centered in the timber does not
lower the grade .... defects(knots) on the faces
are what influence grade the most.

In a situation where two timbers (5X8's) can be
sawn from the log/stem, is there a preferred
or recommended approach? My first instinct would
be to saw either timber a bit away from the pith
to avoid having the associated pith defects on
the face of the timber - in essence, sawing a
thin plank that contains the pith, from the center
of the log.

As and aside, I believe I've read in one of the
FPL documents that anything 5" or wider can be/is
considered a timber ...

Thoughts appreciated

Carl

4/7/20       #2: Sawing timbers for maximum strength ...
rich c.

Boxed heart will give you the best result for straight beams. After that it depends on the tree. No exact science that I know of.

4/8/20       #3: Sawing timbers for maximum strength ...
Keith Newton

Carl, I think if it were up to me, and I may be doing the same for a structure for myself before long, I would put the pith side up. I would also be tempted to do a rip cut down the length aligned with the pith. This might relieve the stress to check on the other 3 visible sides, and wouldn’t have any effect on the strength in that orientation.

Is that 10’ the full length of the rafter, or just between braces?

4/8/20       #4: Sawing timbers for maximum strength ...
GeneWengert-WoodDoc

We know that the wood around the pith, sometimes called juvenile wood, shrinks as it dries. If the pith is off center, then you will have a warped beam. So, do everything you can to center the pith exactly, end to end. If the log is crooked or sweepy, discard it.

4/8/20       #5: Sawing timbers for maximum strength ...
GeneWengert-WoodDoc

Juvenile wood shrinks lengthwise when it dries, while regular wood has close to zero lengthwise shrinkage.

Juvenile wood is also weak, so putting it in the center assures small effect on the overall strength.

4/9/20       #6: Sawing timbers for maximum strength ...
Carl

OK - I think I've got a handle on this now,
and thanks to all who replied.

My take away is that if sawing timbers for the
highest strength/grade is the goal, then choosing
straight logs and accurately centering the pith
will produce the highest rated timbers.

I was aware that the juvenile wood that surrounds
the pith shrank considerably more then non-juvenile
wood, but wasn't aware that is was also weaker.
Centering the pith would make sense, since it would
place the weaker juvenile wood at the neutral axis
of the beam, where stresses are the lowest. And
since timbers can't realistically be dried to
inservice MC before installing them, centering the
pith sure seems like it would go a long ways
towards equalizing the shrinkage around the timber.

Rather then try and squeeze two timbers out of the
larger logs, I'm going to first try and use up any
smaller diameter logs, and then "saw around" the
larger ones until I've got a cant to saw the beam
from.

also - as to the question: "Is that 10’ the full length
of the rafter, or just between braces?" the unsupported
span of the rafter is 10' - the overall length will
be 14 to 16 feet.

Carl

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Rose Machinery
      Horizontal Band Re-rips, Standard & Custom Designed Machinery
    • Baker Products
      Industrial Woodworking Machines, Wooden Pallet Manufacturing Machines, & Portable Sawmills

    Become a Sponsor today!