Sawing and Drying

You are not logged in. [ Login ] Why log in
(NOTE: Login is not required to post)

Post a Response
The staff at WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at any WOODWEB Forum. Participants should undertake the use of machinery, materials and methods discussed after considerate evaluation, and at their own risk.
Your Name:
Your Website:
Email Address:
Subject:

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Drying mixed species (ash/cherry) in a solar kiln

6/25/20       
Carl

I've been sawing and drying thousands of feet of
ash over the last couple of years, and have gotten
very familiar with its behavior in my solar kiln.
Even at this time of year (late June), when the
kiln performs at its best, I haven't had any issues
with a "too fast" drying rate. My typical loads are
500-600 ft of 8-10 foot lengths of 4/4 lumber.

In this next batch, I have a cherry tree that was
uprooted in a storm a few weeks ago that I'd like
to include, and recognize that the max drying rate
for cherry is much much slower then ash. Ash is listed
at 10-1/2% per day while cherry is just under 6%.

I have some thoughts on how to approach this, and
would appreciate input/suggestions ....

1) cover about half of the kiln roof to slow the
drying rate. Covering the roof will be a bit of a
pain, but I'm just wondering if the two approaches
below have merit - they'd certainly be easier.

2) reduce fan speed - I use three, 3 speed fans
and typically run them all at the fastest setting.
I could run them at the lowest speed .... this would
certainly be the easiest approach.

3) put the cherry on the bottom of the stack and
partially block the horizontal sticker gaps to
slow the airflow only around the cherry. This would
allow the rest of the load to dry at the normal rate
while slowing down just the cherry.

Some additional questions .....

Q1) In a normal load, if cherry and ash were mixed,
would monitoring the drying rate for ash
samples provide current info on the rate
of loss for the cherry? In other words,
with kiln conditions the same for both, would
they loss moisture at the same rate?

Q2) in any of the methods, does damage from a
too-fast rate start immediately, or is there
any kind of grace period? How would one day at a
too-fast rate compare to 2, 4, 6 days? I can
monitor the rate daily

Q3) is there a MC point where the drying rate for
cherry can be accelerated without risk? I've
read over the years that once MC reaches mid/low
20's, potential drying problems are greatly
reduced ... maybe even gone?

I hope to use this round of drying as to hopefully
come up with the best way to dry mixed species in
a load. I don't saw at any volume, and can see
that there could be instances in the future where
mixed loads would be an advantage. Any thoughts
on the over all aspect of drying mixed species
is appreciated

Carl


View higher quality, full size image (1200 X 800)

2/23/22       #2: Drying mixed species (ash/cherry) i ...
Carter Asco

The sheets alone are not useful as a vapor barrier, as moisture can get around the edges. Special sealing is required for the edges when two panels join or the panel is in contact with wood framing.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Carter Products
      Band Saw Guides, Blades, Wheels, Tires, Line Lasers and 2D Projectors, Wide Belt Sanding Accessories, Vacuum Holding Systems and More
    • Baker Products
      Industrial Woodworking Machines, Wooden Pallet Manufacturing Machines, & Portable Sawmills
    • Rose Machinery
      Horizontal Band Re-rips, Standard & Custom Designed Machinery

    Become a Sponsor today!