Belt Sander thickness tolerances

9/19/18       
Craig Caughlan Member

Website: wetimber.mx

I’m curious as to what others think are acceptable tolerances in belt sanders.

I’m running 3” x 3” x 12’ laminated stock and experiencing a variation of 0.3mm along the length. I’ve 8’ extension tables in the infeed & outfeed.

9/19/18       #2: Belt Sander thickness tolerances ...
Craig Caughlan Member

Website: wetimber.mx

I was not clear; the 0.3mm difference varies along the length.

9/20/18       #3: Belt Sander thickness tolerances ...
bill Member

What type of sander? How much material are you trying to remove?

9/20/18       #4: Belt Sander thickness tolerances ...
Craig Caughlan Member

Website: wetimber.mx

Haha. I didn't want to mention the sander so as not to prejudice the response. It's a new JET 16-32. I know it's hardly industrial. We're removing 0.5mm on pino radiata using 100 grit. The drum is absolutely parallel to the table, and my outfeed tables are dead level. I can run two sticks through at the same place and get variations from 0-0.3mm in the same locations. And of course, even this would change slightly as the abrasive wears.

It made me curious as to what are acceptable tolerances.

9/20/18       #5: Belt Sander thickness tolerances ...
bill Member

That's not a belt sander its a drum sander.

We have an 8,000 pound Butfering and we will only remove .3mm per pass with 2 heads so perhaps you are being a little aggressive.

You might want to try 0.1mm or less and make sure your outfeed and outfeed table is doing the job correctly.

9/20/18       #6: Belt Sander thickness tolerances ...
Craig Caughlan Member

Website: wetimber.mx

Wow! So 0.1mm is your tolerance - 0.004"?
That's incredible; I thought those kind of tolerances were only in metal fabrication. I would not of thought in wood.

9/20/18       #7: Belt Sander thickness tolerances ...
bill Member

Sorry I meant we remove .3mm per pass. You might want to remove .1 mm per pass or less to get a better result.

A sander, especially a drum sander is not meant to be a planer. If you put in a piece that has that variation it will come out with that variation. A good sander will remove an equal amount of material along the length. The drum is padded the belt will compress. Grits of sandpaper are only capable of removing a certain amount of material. Your expectation is very high for that piece of equipment.

9/20/18       #8: Belt Sander thickness tolerances ...
Bryan "doc" Henderson  Member

If you have access to a jointer, it could take the variation out, then of course plane the opposite sides to be parallel. 0.3 mm is tiny. What role do these pieces play in your project

9/20/18       #9: Belt Sander thickness tolerances ...
Bryan "doc" Henderson  Member

As it is laminated, I would expect the density to be fairly uniform. The cantilever design, if I am thinking of the correct sander, can flex a little. Those are good sized pieces. Good luck

9/21/18       #10: Belt Sander thickness tolerances ...
Adam West  Member

Website: http://www.surfprepsanding.com

.5mm is over the maximum that 100 grit can remove in perfect conditions.. 4mm is pushing the maximum. I wouldn't take any more than .3mm on that drum sander.

You will always get some thickness deviation due to warp or twist in the board. Not much you can do about that.

9/22/18       #11: Belt Sander thickness tolerances ...
Craig Caughlan Member

Website: wetimber.mx

The laminated stock is for rails & stiles of large shutters that we're fabricating. We bought the drum sander to do the slats, which we have 6,000 of. I was curious as to how this machine would handle the stile stock. Thanks for your comments.

2/5/19       #12: Belt Sander thickness tolerances ...
Paul M. Member

Wait, what side has the 0.3 cm variation? Using a drum sander can result in this, you might want to use a belt sander instead.

  • Post a Response to this thread
  • notify me of responses to this topic
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors

    Become a Sponsor today!